A method for preparing phenolic epoxy fiber by melt spinning
By combining the phenolic resin and epoxy resin generated by the reaction under acidic and alkaline conditions, the melt spinning and microwave curing methods are used to prepare the phenolic epoxy fiber, which solves the problems of complexity and pollution of the existing phenolic spinning process and improves the efficiency of the existing phenolic spinning process. The flame retardancy and mechanical properties of the fiber enable simplified processes and the possibility of mass production.
Patent Information
- Application Number
- CN202310683223.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-09
AI Technical Summary
The existing phenolic spinning process is complex and pollutes the environment, making it difficult to produce on a large scale, and the phenolic fiber is brittle and has insufficient spinning performance.
Phenols and aldehydes are reacted under acidic conditions to generate high-ortho-positioned thermoplastic phenolic resin, and reacted with alcohols under alkaline conditions to generate thermosetting phenolic resin. After mixing, they are melt-spun and microwave-cured with epoxy resin to prepare Flame-retardant, heat-resistant phenolic epoxy fiber.
It simplifies the process flow, reduces pollution, improves the flame retardancy, heat resistance and mechanical properties of phenolic epoxy fiber, solves the problems of traditional phenolic fiber being brittle and difficult to spin, and is suitable for a wide range of application fields.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of special fibers, and particularly relates to a method for preparing phenolic epoxy fibers by melt spinning. Background Art
[0002] Phenolic resin is the world's first industrialized synthetic resin, boasting over 100 years of history. Its products possess unique properties, including heat resistance, flame retardancy, electrical insulation, mechanical properties, and dimensional stability. Phenolic fiber, a novel organic fiber material obtained through spinning, neither melts nor burns in a 2500°C flame, only carbonizing and retaining its original fiber state. Furthermore, it exhibits excellent thermal insulation properties under ablation conditions and exhibits excellent corrosion resistance to various acids and organic solvents. Consequently, it is widely used in fire-resistant fibers and specialty clothing.
[0003] Li Jianhua (Application No. 202010413507.5, a method for preparing phenolic fiber) produces phenolic primary fiber by melt spinning phenolic resin, and then crosslinks it in a curing solution composed of formaldehyde, hydrochloric acid, and deionized water, and then produces phenolic fiber by high-temperature crosslinking treatment. However, the curing process for preparing phenolic fiber is cumbersome, and the curing solution is difficult to handle and pollutes the environment. The present invention produces phenolic epoxy resin by using epoxy resin blending, and produces phenolic epoxy fiber by melt spinning and microwave curing. Summary of the Invention
[0004] Aiming at the technical and pollution problems existing in the existing phenolic spinning process, the present invention proposes a method for preparing phenolic epoxy fiber by melt spinning technology. The method has the characteristics of simple process, low pollution, short production cycle, and the prepared phenolic epoxy fiber has excellent flame retardant and heat insulation properties.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] The invention comprises the following steps: reacting phenols and aldehydes under acidic conditions to generate high-ortho-thermoplastic phenolic resins; reacting the high-ortho-thermoplastic phenolic resins, aldehydes and alcohols under alkaline conditions to generate a thermosetting phenolic resin solution; mixing the thermosetting phenolic resin solution and an epoxy resin to obtain a melt spinning solution; melt spinning to obtain nascent fibers; and then subjecting the fibers to microwave curing to obtain flame-retardant and heat-resistant phenolic epoxy fibers prepared by melt spinning.
[0007] The specific preparation method is as follows:
[0008] A method for preparing phenolic epoxy fiber by melt spinning, comprising the following steps:
[0009] (1) Phenol is mixed with formaldehyde and a divalent metal salt catalyst for reaction, heated to boiling and maintained for 3.5-4.5 hours, an acidic catalyst is added to adjust the pH value to acidic, the reaction is carried out for 0.5-1.5 hours, and vacuum distillation is performed to a minimum temperature of 35-45°C, and then the temperature is gradually increased to 110°C at a rate of 0.1-2°C / min to produce a high-ortho-thermoplastic phenolic resin;
[0010] (2) The high-ortho-thermoplastic phenolic resin in (1) is mixed with an aldehyde compound and an alcohol compound, and sodium hydroxide is adjusted to alkaline and heated to 45-60°C and maintained for 0.5-2h, and then heated to 80-95°C and reacted for 6-8h. After the reaction solution cools to room temperature, sulfuric acid is added to adjust the pH to neutral, and the solution is centrifuged or filtered under reduced pressure, and dried at low temperature to remove the water therein to obtain an alcohol-soluble phenolic resin solution;
[0011] (3) mixing the alcohol-soluble phenolic resin solution with the epoxy resin compound, heating to 60-80°C, and distilling under reduced pressure to obtain a molten spinning solution;
[0012] (4) The obtained spinning solution is melt-spinned to prepare primary fibers, and the primary fibers are heat-cured to obtain phenolic epoxy fibers.
[0013] The divalent metal salt catalyst in step (1) is barium acetate.
[0014] In step (1), the molar ratio of phenol to formaldehyde is 1:(0.75-0.9), and the molar ratio of phenol to divalent metal salt catalyst is 1:(0.01-0.02).
[0015] The pressure of the reduced pressure distillation in step (1) is 0.001-0.002 MPa.
[0016] In step (2), the aldehyde compound is formaldehyde or acetaldehyde; and the alcohol compound is methanol, ethanol, propylene glycol or n-butanol.
[0017] In the step (2), the molar ratio of the high-ortho thermoplastic phenolic compound to the aldehyde compound is 1:(4-8); and the mass ratio of the aldehyde compound to the alcohol compound is 1:(1.8-5.5).
[0018] The pressure of the reduced pressure filtration in step (2) is 0.001-0.01 MPa.
[0019] In step (3), the epoxy resin compound is epoxy resin F44 or F704, the mass ratio of alcohol-soluble phenolic resin solution:epoxy resin compound is 1:(0.05-1.2), and the pressure of reduced pressure distillation is 0.0015-0.01 MPa.
[0020] In the step (4), the obtained spun fibers are heated to 150-190° C. in air and kept at this temperature for 10-20 minutes for heat curing.
[0021] The beneficial effects of the present invention are:
[0022] The present invention uses a barium acetate catalyst, which is beneficial for removing the catalyst after pH adjustment in the later stage, thereby improving the stability of the final resin; the main method for preparing phenolic epoxy fiber adopts the melt spinning method, which solves the disadvantages of other spinning methods such as long production cycle and difficulty in large-scale production; the use of thermal curing treatment can further improve the flame retardancy and heat resistance of phenolic epoxy fiber; the use of epoxy resin can improve the brittleness, adhesion and heat resistance of phenolic resin. The nascent fibers obtained by melt spinning generally need to be cured with the help of a curing agent, or cross-linked using a hydrochloric acid-formaldehyde curing solution, but are prone to produce carcinogenic dichloromethyl ether, which pollutes the environment. The present patent uses a thermosetting phenolic epoxy resin to solve the problems of complex processes brought about by traditional curing methods. By achieving a high molecular weight of thermosetting phenolic resin through high ortho-position hydroxymethylation, and simultaneously adding epoxy resin to the thermosetting phenolic resin, a phenolic-epoxy melt with phenolic resin as the main chain and epoxy as the side chains is formed in the spinning solution. This increases the molecular chain length, the distance between the chains, and the flexibility of the chains, thus resolving the inherent difficulty in spinning and brittleness of phenolic fiber. The epoxy cross-linking reaction eliminates the release of small molecules, which improves the density of the fiber after curing and promotes the improvement of the fiber's mechanical properties. The prepared phenolic-epoxy fiber has the advantages of flame retardancy, high temperature resistance, high strength, good toughness, and corrosion resistance, and has a wide range of applications. DETAILED DESCRIPTION
[0023] The present invention will be further described below with reference to specific examples. It should be understood that the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention, and that those skilled in the art may make non-essential improvements and adjustments based on the contents of the above invention. Example 1
[0024] This embodiment provides a method for preparing phenolic epoxy fiber by melt spinning, the steps of which are as follows: (1) phenol and formaldehyde are mixed in a molar ratio (1:0.75) and a catalyst of barium acetate (the mass ratio of phenol to divalent metal salt is 1:0.01) for reaction, and the mixture is heated until the solution boils and maintained for 3.5 hours. Sulfuric acid is added to adjust the pH value to acidic. After reacting for 0.5 hours, the mixture is depressurized to a minimum temperature of 35°C at 0.001 MPa, and then the temperature is gradually increased to 110°C at a rate of 0.1°C / min under reduced pressure to generate a high-ortho-thermoplastic phenolic resin.
[0025] (2) Mix high-ortho-thermoplastic phenolic resin with formaldehyde and methanol (the molar ratio of high-ortho-thermoplastic phenolic resin to aldehyde compound is 1:4, and the molar ratio of aldehyde compound to alcohol compound is 1:1.8), add sodium hydroxide to adjust to alkalinity, heat to 45°C and maintain for 0.5h, then heat to 80°C and react for 6h. After the reaction solution cools to room temperature, add sulfuric acid to adjust the pH to neutral, filter under reduced pressure at 0.001MPa, and dry at low temperature to remove water therein to obtain an alcohol-soluble phenolic resin solution.
[0026] (3) The alcohol-soluble phenolic resin solution and the epoxy resin F44 were mixed in a mass ratio of 1:0.05, heated to 60°C and distilled under reduced pressure at a pressure of 0.001 MPa. The molten spinning stock solution was placed in a melt spinning machine for melt spinning. The obtained nascent fibers were heated to 150°C in an air environment and kept warm for 10 minutes to obtain phenolic fibers prepared by the melt spinning method.
[0027] The experimental results show that the obtained phenolic fiber has a limiting oxygen index of 34, an elongation at break of 50%, a tensile strength of 7.3 cN / dtex, a residual carbon rate of 58% under a nitrogen atmosphere at 900°C, a modulus of 42 cN / dtex, and a thermal decomposition temperature of 260°C. Example 2
[0028] This embodiment provides a method for preparing phenolic epoxy fiber by melt spinning, the steps are as follows:
[0029] (1) Phenol and formaldehyde were mixed in a molar ratio of 1:0.9 and a catalyst of barium acetate (the mass ratio of phenol to divalent metal salt was 1:0.02) and heated to boiling for 4.5 h. Sulfuric acid was added to adjust the pH to acidic. After 1.5 h of reaction, the pressure was reduced to 45°C at 0.002 MPa and then gradually heated to 110°C at 2°C / min under reduced pressure to generate a high-ortho-thermoplastic phenolic resin.
[0030] (2) High-ortho-thermoplastic phenolic resin is mixed with acetaldehyde and ethanol (the molar ratio of high-ortho-thermoplastic phenolic resin to aldehyde compound is 1:8, and the molar ratio of aldehyde compound to alcohol compound is 1:5.5). Sodium hydroxide is adjusted to alkaline and heated to 60°C for 2 hours, then heated to 95°C for 8 hours. After the reaction solution cools to room temperature, sulfuric acid is added to adjust the pH to neutral, centrifuge, and dry at low temperature to remove water therein to obtain an alcohol-soluble phenolic resin solution.
[0031] (3) The alcohol-soluble phenolic resin solution and the epoxy resin F704 were mixed in a mass ratio of 1:1.2, heated to 80°C and distilled under reduced pressure at a pressure of 0.01 MPa. The molten spinning stock solution was placed in a melt spinning machine for melt spinning. The obtained nascent fibers were heated to 190°C in an air environment and kept warm for 20 minutes to obtain phenolic fibers prepared by the melt spinning method.
[0032] The experimental results show that the obtained phenolic fiber has a limiting oxygen index of 34, an elongation at break of 60%, a tensile strength of 7.3 cN / dtex, a residual carbon rate of 58% under a nitrogen atmosphere at 900°C, a modulus of 42 cN / dtex, and a thermal decomposition temperature of 260°C. Example 3
[0033] This embodiment provides a method for preparing phenolic epoxy fiber by melt spinning, the steps are as follows:
[0034] (1) Phenol and formaldehyde were mixed in a molar ratio of 1:0.85 and a catalyst of barium acetate (the mass ratio of phenol to divalent metal salt was 1:0.01) and heated to boiling for 3.5 h. Sulfuric acid was added to adjust the pH to acidic. After reacting for 0.5 h, the temperature was reduced to 40°C at 0.002 MPa and then gradually increased to 110°C at a rate of 0.1°C / min under reduced pressure to generate a high ortho-thermoplastic phenolic resin.
[0035] (2) High-ortho-thermoplastic phenolic resin is mixed with formaldehyde and propylene glycol (the molar ratio of high-ortho-thermoplastic phenolic resin to aldehyde compound is 1:4, and the molar ratio of aldehyde compound to alcohol compound is 1:1.8). Sodium hydroxide is adjusted to alkaline and heated to 45°C for 0.5h. The temperature is then raised to 80°C for reaction for 6h. After the reaction solution cools to room temperature, sulfuric acid is added to adjust the pH to neutral. The solution is filtered under reduced pressure at 0.001MPa and dried at low temperature to remove the water therein to obtain an alcohol-soluble phenolic resin solution.
[0036] (3) The alcohol-soluble phenolic resin solution and the epoxy resin F704 were mixed in a mass ratio of 1:0.05, heated to 60°C and distilled under reduced pressure at a pressure of 0.01 MPa. The molten spinning stock solution was placed in a melt spinning machine for melt spinning. The obtained nascent fibers were heated to 150°C in an air environment and kept warm for 10 minutes to obtain phenolic fibers prepared by the melt spinning method.
[0037] The experimental results show that the phenolic fiber has a limiting oxygen index of 34, an elongation at break of 56%, a tensile strength of 8.3 cN / dtex, a residual carbon rate of 58% under a nitrogen atmosphere at 900°C, a modulus of 42 cN / dtex, and a thermal decomposition temperature of 260°C. Example 4
[0038] This embodiment provides a method for preparing phenolic epoxy fiber by melt spinning, the steps are as follows
[0039] (1) Phenol and formaldehyde were mixed in a molar ratio of 1:0.85 and a catalyst of barium acetate (the mass ratio of phenol to divalent metal salt was 1:0.01) and heated to boiling for 3.5 hours. Sulfuric acid was added to adjust the pH to acidic. After reacting for 0.5 hours, the temperature was reduced to 40°C at 0.002 MPa and then gradually increased to 110°C at a rate of 0.1°C / min under reduced pressure to generate a high ortho-thermoplastic phenolic resin.
[0040] (2) High-ortho-thermoplastic phenolic resin is mixed with formaldehyde and n-butanol (the molar ratio of high-ortho-thermoplastic phenolic resin to aldehyde compound is 1:6, and the molar ratio of aldehyde compound to alcohol compound is 1:4). Sodium hydroxide is adjusted to alkaline and heated to 55°C for 1.5 hours. The temperature is then raised to 85°C for reaction for 6 hours. After the reaction solution cools to room temperature, sulfuric acid is added to adjust the pH to neutral. The solution is filtered under reduced pressure at 0.008 MPa and dried at low temperature to remove the water therein to obtain an alcohol-soluble phenolic resin solution.
[0041] (3) The alcohol-soluble phenolic resin solution and the epoxy resin F44 were mixed in a mass ratio of 1:1, heated to 70°C and distilled under reduced pressure at a pressure of 0.0015 MPa. The molten spinning stock solution was placed in a melt spinning machine for melt spinning. The obtained nascent fibers were heated to 170°C in an air environment and kept warm for 15 minutes to obtain phenolic fibers prepared by the melt spinning method.
[0042] The experimental results show that the phenolic fiber obtained has a limiting oxygen index of 31, an elongation at break of 67%, a tensile strength of 5.3 cN / dtex, a residual carbon rate of 56% under a nitrogen atmosphere at 900°C, a modulus of 35 cN / dtex, and a thermal decomposition temperature of 270°C. Example 5
[0043] This embodiment provides a method for preparing phenolic epoxy fiber by melt spinning, the steps are as follows
[0044] (1) Phenol and formaldehyde were mixed in a molar ratio of 1:0.85 and a catalyst of barium acetate (the mass ratio of phenol to divalent metal salt was 1:0.01) and heated to boiling for 3.5 hours. Sulfuric acid was added to adjust the pH to acidic. After reacting for 0.5 hours, the temperature was reduced to 40°C at 0.002 MPa and then gradually increased to 110°C at a rate of 0.1°C / min under reduced pressure to generate a high ortho-thermoplastic phenolic resin.
[0045] (2) High-ortho-thermoplastic phenolic resin is mixed with formaldehyde and n-butanol (the molar ratio of high-ortho-thermoplastic phenolic resin to aldehyde compound is 1:6, and the molar ratio of aldehyde compound to alcohol compound is 1:5). Sodium hydroxide is adjusted to alkaline and heated to 55°C for 1.5 hours. The temperature is then raised to 85°C for reaction for 6 hours. After the reaction solution cools to room temperature, sulfuric acid is added to adjust the pH to neutral. The solution is filtered under reduced pressure at 0.008 MPa and dried at low temperature to remove the water therein to obtain an alcohol-soluble phenolic resin solution.
[0046] (3) The alcohol-soluble phenolic resin solution and the epoxy resin F704 were mixed in a mass ratio of 1:1.1, heated to 70°C and distilled under reduced pressure at a pressure of 0.007 MPa. The molten spinning stock solution was placed in a melt spinning machine for melt spinning. The obtained nascent fibers were heated to 170°C in an air environment and kept warm for 15 minutes to obtain phenolic fibers prepared by the melt spinning method.
[0047] The experimental results show that the phenolic fiber obtained has a limiting oxygen index of 30, an elongation at break of 77%, a tensile strength of 3.3 cN / dtex, a residual carbon rate of 56% under a nitrogen atmosphere at 900°C, a modulus of 19 cN / dtex, and a thermal decomposition temperature of 280°C. Example 6
[0048] This embodiment provides a method for preparing phenolic epoxy fiber by melt spinning, the steps are as follows:
[0049] (1) Phenol and formaldehyde were mixed in a molar ratio of 1:0.86 and a catalyst of barium acetate (the mass ratio of phenol to divalent metal salt was 1:0.01), and the solution was heated to boiling for 3.5 hours. Sulfuric acid was added to adjust the pH to acidic. After reacting for 0.5 hours, the temperature was reduced to 40°C at 0.002 MPa, and then the temperature was gradually increased to 110°C at a rate of 0.1°C / min under reduced pressure to generate a high-ortho-thermoplastic phenolic resin.
[0050] (2) High-ortho-thermoplastic phenolic resin is mixed with formaldehyde and n-butanol (the molar ratio of high-ortho-thermoplastic phenolic resin to aldehyde compound is 1:7, and the molar ratio of aldehyde compound to alcohol compound is 1:5). Sodium hydroxide is adjusted to alkaline and heated to 55°C for 1.5 hours. The temperature is then raised to 85°C for reaction for 6 hours. After the reaction solution cools to room temperature, sulfuric acid is added to adjust the pH to neutral. The solution is filtered under reduced pressure at 0.008 MPa and dried at low temperature to remove the water therein to obtain an alcohol-soluble phenolic resin solution.
[0051] (3) The alcohol-soluble phenolic resin solution and the epoxy resin F704 were mixed in a mass ratio of 1:0.9, heated to 74°C and distilled under reduced pressure at a pressure of 0.007 MPa. The molten spinning stock solution was placed in a melt spinning machine for melt spinning. The obtained nascent fibers were heated to 170°C in an air environment and kept warm for 15 minutes to obtain phenolic fibers prepared by the melt spinning method.
[0052] The experimental results show that the phenolic fiber has a limiting oxygen index of 31, an elongation at break of 79%, a tensile strength of 4.3 cN / dtex, a residual carbon rate of 66% under a nitrogen atmosphere at 900°C, a modulus of 19 cN / dtex, and a thermal decomposition temperature of 284°C. Example 7
[0053] This embodiment provides a method for preparing phenolic epoxy fiber by melt spinning, the steps are as follows:
[0054] (1) Phenol and formaldehyde were mixed in a molar ratio of 1:0.85 and a catalyst of barium acetate (the mass ratio of phenol to divalent metal salt was 1:0.02), and the solution was heated to boiling for 3.5 hours. Sulfuric acid was added to adjust the pH to acidic. After reacting for 0.5 hours, the temperature was reduced to 40°C under 0.002 MPa, and then the temperature was gradually increased to 110°C at a rate of 0.1°C / min under reduced pressure to generate a high-ortho-thermoplastic phenolic resin.
[0055] (2) High-ortho-thermoplastic phenolic resin is mixed with formaldehyde and n-butanol (the molar ratio of high-ortho-thermoplastic phenolic resin to aldehyde compound is 1:5, and the molar ratio of aldehyde compound to alcohol compound is 1:5), sodium hydroxide is added to adjust to alkalinity, heated to 55°C and maintained for 1.5 hours, and then heated to 85°C for reaction for 6 hours. After the reaction solution cools to room temperature, sulfuric acid is added to adjust the pH to neutral, and the solution is filtered under reduced pressure at 0.01 MPa and dried at low temperature to remove the water therein to obtain an alcohol-soluble phenolic resin solution.
[0056] (3) The alcohol-soluble phenolic resin solution and the epoxy resin F44 were mixed in a mass ratio of 1:1, heated to 74°C and distilled under reduced pressure at a pressure of 0.007 MPa. The molten spinning stock solution was placed in a melt spinning machine for melt spinning. The obtained nascent fibers were heated to 170°C in an air environment and kept warm for 15 minutes to obtain phenolic fibers prepared by the melt spinning method.
[0057] The experimental results show that the phenolic fiber has a limiting oxygen index of 31, an elongation at break of 72%, a tensile strength of 4.1 cN / dtex, a residual carbon rate of 56% under a nitrogen atmosphere at 900°C, a modulus of 19 cN / dtex, and a thermal decomposition temperature of 274°C.
[0058] The basic principles, main features, and advantages of the present invention are shown and described above. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are merely illustrative of the principles of the present invention. Various changes and modifications may be made to the present invention without departing from the spirit and scope of the present invention. Such changes and modifications are intended to fall within the scope of the present invention. The scope of protection claimed in the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing phenolic epoxy fiber by melt spinning, characterized in that Here are the steps: (1) Mix phenol, formaldehyde and a divalent metal salt catalyst for reaction, heat the solution until it boils and keep boiling for 3.5-4.5 hours, add an acidic catalyst to adjust the pH value to acidic, react for 0.5-1.5 hours, distill under reduced pressure to a minimum temperature of 35-45°C, and gradually increase the temperature to 110°C at a rate of 0.1-2°C / min to generate a high ortho-thermoplastic phenolic resin; (2) mixing the high-ortho-thermoplastic phenolic resin in step (1) with an aldehyde compound and an alcohol compound, adjusting the sodium hydroxide to alkalinity, heating to 45-60° C. and maintaining for 0.5-2 h, raising the temperature to 80-95° C., reacting for 6-8 h, and after the reaction solution cools to room temperature, adding sulfuric acid to adjust the pH to neutral, centrifuging or filtering under reduced pressure, and drying at low temperature to remove water therein to obtain an alcohol-soluble phenolic resin solution; (3) mixing the alcohol-soluble phenolic resin solution with the epoxy resin compound, heating to 60-80° C., and distilling under reduced pressure to obtain a molten spinning solution; (4) preparing primary fibers from the obtained spinning solution by a melt spinning method, and performing a heat curing treatment on the primary fibers to obtain phenolic epoxy fibers; In the step (3), the epoxy resin compound is epoxy resin F44 or F704, the mass ratio of alcohol-soluble phenolic resin solution:epoxy resin compound is 1:(0.05-1.2), and the pressure of reduced pressure distillation is 0.0015-0.01 MPa.
2. The method for preparing phenolic epoxy fiber by melt spinning according to claim 1, characterized in that: The divalent metal salt catalyst in step (1) is barium acetate.
3. The method for preparing phenolic epoxy fiber by melt spinning according to claim 1, characterized in that: In the step (1), the molar ratio of phenol to formaldehyde is 1:(0.75-0.9), and the molar ratio of phenol to divalent metal salt catalyst is 1:(0.01-0.02).
4. The method for preparing phenolic epoxy fiber by melt spinning according to claim 1, characterized in that: The pressure of the reduced pressure distillation in step (1) is 0.001-0.002 MPa.
5. The method for preparing phenolic epoxy fiber by melt spinning according to claim 1, characterized in that: In step (2), the aldehyde compound is formaldehyde or acetaldehyde; the alcohol compound is methanol, ethanol, propylene glycol or n-butanol.
6. The method for preparing phenolic epoxy fiber by melt spinning according to claim 1, characterized in that: In the step (2), the molar ratio of the high-ortho-thermoplastic phenolic acid to the aldehyde compound is 1:(4-8); and the mass ratio of the aldehyde compound to the alcohol compound is 1:(1.8-5.5).
7. The method for preparing phenolic epoxy fiber by melt spinning according to claim 1, characterized in that: The pressure of the reduced pressure filtration in step (2) is 0.001-0.01 MPa.
8. The method for preparing phenolic epoxy fiber by melt spinning according to claim 1, characterized in that: In the step (4), the obtained nascent fibers are heated to 150-190° C. in air and kept at this temperature for 10-20 minutes for heat curing.
Citation Information
Patent Citations
A method for preparing phenolic fibers
CN111501114B
Epoxy-phenol-formaldehyde resin prepreg and preparation method therefor
CN106167599A
Method for preparing high-ortho thermosetting phenol-formaldehyde fibers by wet spinning
CN109208116A