A method for epoxy resin modified thermosetting high-ortho-phenolic fiber
Through epoxy resin modification and microwave curing technology, the problem of small molecule by-products affecting the performance of phenolic fiber during the curing process has been solved, efficient and environmentally friendly phenolic fiber preparation has been achieved, and the heat resistance, flame retardancy and mechanical properties of the fiber have been improved. Broadened the application fields.
Patent Information
- Application Number
- CN202310684046.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-10
AI Technical Summary
Thermal curing phenolic fibers produce small molecular by-products during the curing process that affect fiber performance, and the solution curing process has problems of environmental pollution and low curing efficiency.
Epoxy resin is used as a modified substance, and high ortho-phenolic fibers are prepared through physical blending and melt spinning methods, and microwave curing is used for cross-linking and solidification, thus avoiding the generation of small molecule by-products and environmental pollution.
The heat resistance, flame retardancy and mechanical properties of the fiber are improved, the structure is dense and without holes, the curing process is simplified, the curing efficiency is improved, and it is green and environmentally friendly.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of flame-retardant, heat-resistant and corrosion-resistant special fibers, and specifically relates to a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin. Background Art
[0002] Phenolic fiber is widely used in aerospace, industrial construction, transportation and flame-retardant fabrics due to its excellent flame retardancy, heat resistance and corrosion resistance. It can also be processed into porous carbon materials and then applied to adsorption, sensing and other fields.
[0003] However, thermosetting phenolic resin contains phenolic hydroxyl groups, which will generate small molecular water during the curing and cross-linking reaction, causing holes inside the fiber, thereby affecting the various properties of the fiber. Therefore, it is necessary to modify the fiber to be addition curable. Commonly used modified components include epoxy, allyl, propargyl, phenylmaleimide group, BOZ compound, etc. The modified phenolic fiber will undergo addition reaction during cross-linking and curing, and no small molecular by-products will be produced, thus solving the problem of small molecular by-products produced during the curing of phenolic fiber and affecting its performance. At the same time, the introduction of modified substances can improve the heat resistance, flame retardancy, mechanical properties, etc. of the fiber to varying degrees, making phenolic fiber have a wider range of applications.
[0004] Compared with thermoplastic phenolic fiber, thermosetting phenolic fiber can undergo cross-linking and curing reaction without adding curing agent. At the same time, the fiber is post-treated by microwave curing, which effectively avoids the environmental pollution and low curing efficiency caused by the solution curing cross-linking bath.
[0005] The present invention uses epoxy resin as a modifying substance, prepares epoxy-modified thermosetting high-ortho-phenolic epoxy resin by physical blending, prepares fibers by melt spinning, and cross-links and cures the fibers by microwave curing to obtain high-toughness, flame-retardant, and heat-resistant phenolic epoxy fibers. Summary of the invention
[0006] In view of the problems in the prior art that small molecular by-products are produced after the thermosetting phenolic fiber is cured, which affects the fiber performance, and the existing solution curing has serious pollution, the present invention proposes a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin. The prepared phenolic epoxy fiber has excellent flame retardancy, heat resistance and mechanical properties.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] The invention allows phenols and aldehydes to react under metal salt and acidic and alkaline conditions to generate thermoplastic high-ortho-phenolic resin, then reacts the resin with aldehyde compounds under alkaline conditions to generate thermosetting high-ortho-phenolic resin, melt-blended the resin with epoxy resin, and then melt-spun the resulting fibers to obtain primary fibers, which are then subjected to microwave curing treatment to obtain epoxy resin-modified thermosetting high-ortho-phenolic fibers with excellent flame retardancy, heat resistance and mechanical properties.
[0009] The present invention provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, the steps of which are as follows:
[0010] (1) Mixing a phenolic compound, an aldehyde compound and a metal salt catalyst in an oil bath and heating them to keep them in a boiling state for 4-4.5 hours, adding an acidic catalyst and continuing the reaction for 1-1.5 hours, and then placing them in a vacuum distillation device and heating and distilling them to 100-130° C. When the solution is in a viscous state that can be drawn into threads, cooling it to room temperature to obtain a high-ortho-phenolic resin;
[0011] (2) mixing a high-ortho-phenolic resin with an organic solvent, heating at 60-75° C. for 0.5-2 h, adding an alkaline catalyst and an aldehyde compound to continue reacting for 5.5-7 h, cooling to room temperature, and centrifuging to obtain a thermosetting high-ortho-phenolic resin solution;
[0012] (3) adding epoxy resin to the thermosetting high-ortho-phenolic resin solution, heating at 60-75°C for 1-3 hours, removing the organic solvent by vacuum distillation, and heating to 80-95°C for melt spinning to obtain primary fibers;
[0013] (4) The as-spun fibers are microwave cured to obtain epoxy resin-modified thermosetting high-ortho-phenolic fibers.
[0014] The phenolic compound in step (1) is phenol, m-cresol or resorcinol; the aldehyde compound is formaldehyde or acetaldehyde; the metal salt catalyst is barium acetate; and the acid catalyst is hydrochloric acid, oxalic acid or sulfuric acid.
[0015] In the step (1), the molar ratio of the phenolic compound to the aldehyde compound is 1:(0.7-0.9); the mass ratio of the phenolic compound to the metal salt catalyst is 1:(0.01-0.025); and the mass ratio of the phenolic compound to the acidic catalyst is 1:(0.003-0.007).
[0016] During the reduced pressure distillation operation in step (1), the pressure in the device is 0.001-0.0017 MPa; and the heating rate during the reduced pressure distillation operation is 0.08-0.4°C / min.
[0017] In the step (2), the mass ratio of the high-ortho-phenolic resin to the organic solvent is 1:(2-3); the mass ratio of the high-ortho-phenolic resin to the alkaline catalyst is 1:(0.002-0.01); and the mass ratio of the high-ortho-phenolic resin to the aldehyde compound is 1:(0.03-0.3).
[0018] The organic solvent in step (2) is methanol, ethanol or propanol; the alkaline catalyst is sodium hydroxide or barium hydroxide; and the aldehyde compound is formaldehyde or acetaldehyde.
[0019] The centrifugal speed in step (2) is 3500-4500 r / min, and the time is 10-20 min.
[0020] In the step (3), the epoxy resin is E-20 or F-48, the mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin is 1:(0.04-0.5), and the pressure in the device during the reduced pressure distillation operation is 0.001-0.0017 MPa.
[0021] In the step (4), the obtained nascent fibers are placed in a microwave oven under air conditions and subjected to microwave treatment at a power of 60-800 W for 1-30 min.
[0022] The beneficial effects of the present invention are:
[0023] The present invention adopts the method of physical blending to introduce epoxy groups into the phenolic fiber system, and the epoxy groups react with the active hydrogen on the phenol, and no small molecules are generated during the crosslinking process, ensuring that no holes appear in the fiber, which is beneficial to the improvement of fiber performance; the thermosetting phenolic resin can be melt-spun and microwave-cured to complete crosslinking by addition reaction without adding a curing agent; the addition of barium acetate is beneficial to the production of barium sulfate precipitation, which improves the quality of the resin. Compared with the prior art, the raw materials of the present invention are easy to obtain, the modified phenolic fiber has a dense structure and no holes, and its heat resistance, flame retardant performance, mechanical properties, etc. are all improved; by adopting the method of microwave curing, the crosslinking structure inside and outside the fiber is the same, which improves the uniformity of the fiber and overcomes the skin-core structure; at the same time, microwave curing simplifies the curing process, improves the curing efficiency, is green and environmentally friendly, and saves energy, and the epoxy resin modified thermosetting high-ortho-phenolic fiber has the characteristics of flame retardant, heat resistance, corrosion resistance, excellent mechanical properties, etc., which greatly broadens the application field of phenolic fiber. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present invention and are not used to limit the scope of the present invention, and those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention. Example 1
[0025] This embodiment provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, and the steps are as follows:
[0026] (1) Mix phenol, formaldehyde and barium acetate in an oil bath and heat them to keep them in a boiling state for 4 hours, then add sulfuric acid and continue the reaction for 1 hour, then place it in a vacuum distillation device and heat and distill it to 110°C at a heating rate of 0.08°C / min, keeping the pressure in the device at 0.001MPa. When the solution is in a viscous state that can be drawn into threads, pour it out and cool it to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenol:formaldehyde is 1:0.7, the mass ratio of phenol:barium acetate is 1:0.01; the mass ratio of phenol to sulfuric acid is 1:0.003.
[0027] (2) Mix high-ortho-phenolic resin and ethanol, heat at 60°C for 0.5h, add sodium hydroxide and formaldehyde, continue to react for 5.5h, take out, cool to room temperature, and centrifuge at 3500r / min for 10min to obtain thermosetting high-ortho-phenolic resin. The mass ratio of high-ortho-phenolic resin to ethanol is 1:2; the mass ratio of high-ortho-phenolic resin to sodium hydroxide is 1:0.002; and the mass ratio of high-ortho-phenolic resin to formaldehyde is 1:0.03.
[0028] (3) Epoxy resin E-20 was added to the thermosetting high-ortho-phenolic resin solution, heated at 60°C for 1 h, and then the ethanol was removed by vacuum distillation at a pressure of 0.001 MPa. When the solution became viscous, the temperature was raised to 80°C and melt-spun. The resulting nascent fibers were microwave-cured at a power of 60 W for 30 min to obtain phenolic fibers. The mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin was 1:0.04.
[0029] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 36, the elongation at break is 50%, the breaking strength is 3.0 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 59%, the modulus is 20 cN / dtex, and the thermal decomposition temperature under nitrogen is 372°C. Example 2
[0030] This embodiment provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, and the steps are as follows:
[0031] (1) Mix m-cresol, acetaldehyde and barium acetate in an oil bath and heat them to keep them in a boiling state for 4.5 hours, then add hydrochloric acid and continue the reaction for 1.5 hours, then place it in a vacuum distillation device and heat and distill it to 130°C at a heating rate of 0.4°C / min, keeping the pressure in the device at 0.0017MPa. When the solution is in a viscous state that can be drawn into threads, pour it out and cool it to room temperature to obtain a high ortho-phenolic resin. The molar ratio of m-cresol to acetaldehyde is 1:0.9, the mass ratio of m-cresol to barium acetate is 1:0.025, and the mass ratio of phenol to hydrochloric acid is 1:0.007.
[0032] (2) Mix high-ortho-phenolic resin and methanol, heat at 75°C for 2 hours, add barium hydroxide and acetaldehyde, continue to react for 7 hours, take out, cool to room temperature, and centrifuge at 4500r / min for 20 minutes to obtain thermosetting high-ortho-phenolic resin. The mass ratio of high-ortho-phenolic resin to methanol is 1:3; the mass ratio of high-ortho-phenolic resin to barium hydroxide is 1:0.01; and the mass ratio of high-ortho-phenolic resin to acetaldehyde is 1:0.3.
[0033] (3) Epoxy resin F-48 was added to the thermosetting high-ortho-phenolic resin solution, heated at 75°C for 3 h, and then the methanol was removed by vacuum distillation at a pressure of 0.0017 MPa. When the solution became viscous, the temperature was raised to 95°C and melt-spun. The resulting nascent fibers were microwave-cured at a power of 800 W for 1 min to obtain phenolic fibers. The mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin was 1:0.5.
[0034] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 31, the elongation at break is 77%, the breaking strength is 7.1 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 49%, the modulus is 16 cN / dtex, and the thermal decomposition temperature under nitrogen is 342°C. Example 3
[0035] This embodiment provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, and the steps are as follows:
[0036] (1) Resorcinol, acetaldehyde and barium acetate were mixed and heated in an oil bath to keep them in a boiling state for 3.5 hours, and then oxalic acid was added and the reaction was continued for 1.2 hours. Then, the mixture was placed in a vacuum distillation apparatus and heated to 120°C at a heating rate of 0.2°C / min, and the pressure in the apparatus was maintained at 0.0015MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high ortho-phenolic resin. The molar ratio of resorcinol to acetaldehyde was 1:0.8, the mass ratio of m-cresol to barium acetate was 1:0.02, and the mass ratio of phenol to oxalic acid was 1:0.005.
[0037] (2) Mix high-ortho-phenolic resin and propanol, heat at 70°C for 1.5 hours, add barium hydroxide and acetaldehyde, continue to react for 6 hours, take out, cool to room temperature, and centrifuge at 4000r / min for 20 minutes to obtain thermosetting high-ortho-phenolic resin. The mass ratio of high-ortho-phenolic resin to propanol is 1:2.5; the mass ratio of high-ortho-phenolic resin to barium hydroxide is 1:0.008; and the mass ratio of high-ortho-phenolic resin to acetaldehyde is 1:0.1.
[0038] (3) Epoxy resin F-48 was added to the thermosetting high-ortho-phenolic resin solution, heated at 70°C for 2 h, and then the methanol was removed by vacuum distillation at a pressure of 0.0013 MPa. When the solution became viscous, the temperature was raised to 90°C and melt-spun. The resulting nascent fibers were microwave-cured at a power of 600 W for 10 min to obtain phenolic fibers. The mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin was 1:0.3.
[0039] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 32, the elongation at break is 68%, the breaking strength is 2.1 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 48%, the modulus is 21 cN / dtex, and the thermal decomposition temperature under nitrogen is 382°C. Example 4
[0040] This embodiment provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, and the steps are as follows:
[0041] (1) Resorcinol, acetaldehyde and barium acetate were mixed and heated in an oil bath to keep them in a boiling state for 3.5 hours, and then oxalic acid was added and the reaction was continued for 1.2 hours. Then, the mixture was placed in a vacuum distillation apparatus and heated to 120°C at a heating rate of 0.2°C / min, and the pressure in the apparatus was maintained at 0.0015MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high ortho-phenolic resin. The molar ratio of resorcinol to acetaldehyde was 1:0.85, the mass ratio of m-cresol to barium acetate was 1:0.02, and the mass ratio of phenol to oxalic acid was 1:0.005.
[0042] (2) Mix high-ortho-phenolic resin and propanol, heat at 70°C for 1.5 hours, add barium hydroxide and acetaldehyde, continue to react for 6 hours, take out, cool to room temperature, and centrifuge at 4200 r / min for 20 minutes to obtain thermosetting high-ortho-phenolic resin. The mass ratio of high-ortho-phenolic resin to propanol is 1:2.5; the mass ratio of high-ortho-phenolic resin to barium hydroxide is 1:0.008; and the mass ratio of high-ortho-phenolic resin to acetaldehyde is 1:0.1.
[0043] (3) Epoxy resin F-48 was added to the thermosetting high-ortho-phenolic resin solution, heated at 70°C for 2 h, and then the methanol was removed by vacuum distillation at a pressure of 0.0013 MPa. When the solution became viscous, the temperature was raised to 90°C and melt-spun. The nascent fibers were microwave-cured at a power of 600 W for 10 min to obtain phenolic fibers. The mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin was 1:0.4.
[0044] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 32, the elongation at break is 69%, the breaking strength is 3.1 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 48%, the modulus is 29 cN / dtex, and the thermal decomposition temperature under nitrogen is 380°C. Example 5
[0045] This embodiment provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, and the steps are as follows:
[0046] (1) Phenol, formaldehyde and barium acetate were mixed in an oil bath and heated to a boiling state for 4 hours, then sulfuric acid was added and the reaction was continued for 1 hour, and then the mixture was placed in a vacuum distillation apparatus and heated to 110°C at a heating rate of 0.08°C / min, and the pressure in the apparatus was maintained at 0.001MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenol to formaldehyde was 1:0.85, the mass ratio of phenol to barium acetate was 1:0.02, and the mass ratio of phenol to sulfuric acid was 1:0.005.
[0047] (2) Mix high-ortho-phenolic resin and ethanol, heat at 60°C for 0.5h, add sodium hydroxide and formaldehyde, continue to react for 5.5h, take out, cool to room temperature, and centrifuge at 3500r / min for 10min to obtain thermosetting high-ortho-phenolic resin. The mass ratio of high-ortho-phenolic resin to ethanol is 1:2; the mass ratio of high-ortho-phenolic resin to sodium hydroxide is 1:0.002; and the mass ratio of high-ortho-phenolic resin to formaldehyde is 1:0.03.
[0048] (3) Epoxy resin E-20 was added to the thermosetting high-ortho-phenolic resin solution, heated at 60°C for 1 h, and then the ethanol was removed by vacuum distillation at a pressure of 0.001 MPa. When the solution became viscous, the temperature was raised to 80°C and melt-spun. The resulting nascent fibers were microwave-cured at a power of 600 W for 8 min to obtain phenolic fibers. The mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin was 1:0.04.
[0049] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 31, the elongation at break is 80%, the breaking strength is 3.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 53%, the modulus is 19 cN / dtex, and the thermal decomposition temperature under nitrogen is 378°C. Example 6
[0050] This embodiment provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, and the steps are as follows:
[0051] (1) Mix phenol, formaldehyde and barium acetate in an oil bath and heat them to keep them in a boiling state for 4 hours, then add sulfuric acid and continue the reaction for 1.2 hours, then place them in a vacuum distillation apparatus and heat and distill them to 110°C at a heating rate of 0.08°C / min, keeping the pressure in the apparatus at 0.001MPa. When the solution is in a viscous state that can be drawn into threads, pour it out and cool it to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenol to formaldehyde is 1:0.85, the mass ratio of phenol to barium acetate is 1:0.01, and the mass ratio of phenol to sulfuric acid is 1:0.006.
[0052] (2) Mix high-ortho-phenolic resin and ethanol, heat at 60°C for 0.5h, add sodium hydroxide and formaldehyde to continue the reaction for 6h, take out, cool to room temperature, and centrifuge at 3500r / min for 10min to obtain thermosetting high-ortho-phenolic resin. The mass ratio of high-ortho-phenolic resin to ethanol is 1:2; the mass ratio of high-ortho-phenolic resin to sodium hydroxide is 1:0.002; and the mass ratio of high-ortho-phenolic resin to formaldehyde is 1:0.03.
[0053] (3) Epoxy resin F-48 was added to the thermosetting high-ortho-phenolic resin solution, heated at 60°C for 1 h, and then the ethanol was removed by vacuum distillation at a pressure of 0.001 MPa. When the solution became viscous, the temperature was raised to 80°C and melt-spun. The resulting nascent fibers were microwave-cured at a power of 600 W for 9 min to obtain phenolic fibers. The mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin was 1:0.4.
[0054] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 31, the elongation at break is 77%, the breaking strength is 3.8 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 53%, the modulus is 17 cN / dtex, and the thermal decomposition temperature under nitrogen is 371°C. Example 7
[0055] This embodiment provides a method for modifying thermosetting high-ortho-phenolic fiber with epoxy resin, and the steps are as follows:
[0056] (1) Phenol, formaldehyde and barium acetate were mixed and heated in an oil bath to keep them in a boiling state for 4 hours, then sulfuric acid was added and the reaction was continued for 1.2 hours, and then the mixture was placed in a vacuum distillation apparatus and heated to 110°C at a heating rate of 0.08°C / min, and the pressure in the apparatus was maintained at 0.001MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenol to formaldehyde was 1:0.88, the mass ratio of phenol to barium acetate was 1:0.01, and the mass ratio of phenol to sulfuric acid was 1:0.006.
[0057] (2) Mix high-ortho-phenolic resin and ethanol, heat at 60°C for 0.5h, add sodium hydroxide and formaldehyde to continue the reaction for 6h, then take out, cool to room temperature, and centrifuge at 4000r / min for 10min to obtain thermosetting high-ortho-phenolic resin. The mass ratio of high-ortho-phenolic resin to ethanol is 1:2; the mass ratio of high-ortho-phenolic resin to sodium hydroxide is 1:0.002; and the mass ratio of high-ortho-phenolic resin to formaldehyde is 1:0.03.
[0058] (3) Epoxy resin F-48 was added to the thermosetting high-ortho-phenolic resin solution, heated at 60°C for 1 h, and then the ethanol was removed by vacuum distillation at a pressure of 0.001 MPa. When the solution became viscous, the temperature was raised to 80°C and melt-spun. The resulting nascent fibers were microwave-cured at a power of 500 W for 10 min to obtain phenolic fibers. The mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin was 1:0.3.
[0059] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 31, the elongation at break is 79%, the breaking strength is 2.8 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 53%, the modulus is 17 cN / dtex, and the thermal decomposition temperature under nitrogen is 379°C.
[0060] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for epoxy resin modified thermosetting high-ortho phenolic fiber, characterized in that Here are the steps: (1) Mixing a phenolic compound, an aldehyde compound and a metal salt catalyst in an oil bath and heating them to keep them in a boiling state for 4-4.5 hours, adding an acidic catalyst and continuing the reaction for 1-1.5 hours, and then placing them in a vacuum distillation device and heating and distilling them to 100-130° C. When the solution is in a viscous state that can be drawn into threads, cooling it to room temperature to obtain a high-ortho-phenolic resin; (2) mixing a high-ortho-phenolic resin with an organic solvent, heating at 60-75° C. for 0.5-2 h, adding an alkaline catalyst and an aldehyde compound to continue reacting for 5.5-7 h, cooling to room temperature, and centrifuging to obtain a thermosetting high-ortho-phenolic resin solution; (3) adding epoxy resin to the thermosetting high-ortho-phenolic resin solution, heating at 60-75°C for 1-3 hours, removing the organic solvent by vacuum distillation, and heating to 80-95°C for melt spinning to obtain primary fibers; (4) curing the raw fiber by microwave to obtain epoxy resin modified thermosetting high ortho-phenolic fiber; In the step (3), the epoxy resin is E-20 or F-48, the mass ratio of the thermosetting high-ortho-phenolic resin solution to the epoxy resin is 1:(0.04-0.5), and the pressure in the device during the reduced pressure distillation operation is 0.001-0.0017 MPa.
2. The method for modifying thermosetting high-ortho phenolic fiber with epoxy resin according to claim 1, characterized in that: The phenolic compound in step (1) is phenol, m-cresol or resorcinol; the aldehyde compound is formaldehyde or acetaldehyde; the metal salt catalyst is barium acetate; and the acid catalyst is hydrochloric acid, oxalic acid or sulfuric acid.
3. The method for modifying thermosetting high-ortho phenolic fiber with epoxy resin according to claim 1, characterized in that: In the step (1), the molar ratio of the phenolic compound to the aldehyde compound is 1:(0.7-0.9); the mass ratio of the phenolic compound to the metal salt catalyst is 1:(0.01-0.025); and the mass ratio of the phenolic compound to the acidic catalyst is 1:(0.003-0.007).
4. The method for modifying thermosetting high-ortho phenolic fiber with epoxy resin according to claim 1, characterized in that: During the reduced pressure distillation operation in step (1), the pressure in the device is 0.001-0.0017 MPa; and the heating rate during the reduced pressure distillation operation is 0.08-0.4°C / min.
5. The method for modifying thermosetting high-ortho phenolic fiber with epoxy resin according to claim 1, characterized in that: In the step (2), the mass ratio of the high-ortho-phenolic resin to the organic solvent is 1:(2-3); the mass ratio of the high-ortho-phenolic resin to the alkaline catalyst is 1:(0.002-0.01); and the mass ratio of the high-ortho-phenolic resin to the aldehyde compound is 1:(0.03-0.3).
6. The method for modifying thermosetting high-ortho phenolic fiber with epoxy resin according to claim 1, characterized in that: The organic solvent in step (2) is methanol, ethanol or propanol; the alkaline catalyst is sodium hydroxide or barium hydroxide; and the aldehyde compound is formaldehyde or acetaldehyde.
7. The method for modifying thermosetting high-ortho phenolic fiber with epoxy resin according to claim 1, characterized in that: The centrifugal speed in step (2) is 3500-4500 r / min, and the time is 10-20 min.
8. The method for modifying thermosetting high-ortho phenolic fiber with epoxy resin according to claim 1, characterized in that: In the step (4), the obtained nascent fibers are placed in a microwave oven under air conditions and subjected to microwave treatment at a power of 60-800 W for 1-30 min.
Citation Information
Patent Citations
Epoxy-phenol-formaldehyde resin prepreg and preparation method therefor
CN106167599A
Method for preparing high-ortho thermosetting phenol-formaldehyde fibers by wet spinning
CN109208116A