Adhesive for bisque fired blank, adhesive preparation method and ceramic preparation method

By using a specially formulated adhesive to bond bisque-fired ceramic blanks together, the technical challenges of traditional wet ceramic blank bonding have been solved, achieving high bonding strength and efficient production, thereby improving the quality and production efficiency of ceramic products.

CN116655350BActive Publication Date: 2024-11-05SHENZHEN ZHISHAN CERAMIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210156392.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-21
Publication Date
2024-11-05
Estimated Expiration
2042-02-21

Smart Images

  • Figure CN116655350B_ABST
    Figure CN116655350B_ABST
Patent Text Reader

Abstract

The present invention provides an adhesive for bisque fired blanks, an adhesive preparation method and a ceramic preparation method, wherein the adhesive comprises the following components by mass: 40-90 parts of calcined clay; 0.5-10 parts of clay; 0.5-10 parts of calcined kaolin; 0.5-10 parts of flux; 0.5-10 parts of shrinkage stabilizer; 0.5-5 parts of thickener; and 25-35 parts of water. The adhesive for bisque fired blanks of the embodiment of the present invention has a unique formula, good operability, soft glue, high bonding strength, thin adhesive coating, etc., and is sintered after pasting, and the joint is smooth and feels smooth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic preparation, and in particular to an adhesive for bisque fired blanks, an adhesive preparation method and a ceramic preparation method. Background Art

[0002] The parts of traditional ceramic products are pasted together manually by skilled workers who apply wet blank adhesive to the joints of the parts in a wet state. Due to the high water content of the wet blank, insufficient hardness and strength, and uneven manual force, the wet blank parts are easily deformed and have pressing marks, which affects the regularity and overall quality of the product. Therefore, in the process of pasting and pasting, in addition to the high technical requirements for the workers' pasting skills, there will also be shortcomings such as high defective rate and poor overall quality, which seriously affect production efficiency.

[0003] The ceramic green body is placed in a kiln and fired at 750℃ to 850℃ to form a fired body. When the Mohs coefficient reaches 3.5-5.2, the water in the body evaporates, the organic matter burns out, the carbonate decomposes, and the mineral composition and structure are initially formed, so that the body forms a fired body with a certain mechanical strength. The problem of easy deformation and pressing marks of wet body can be solved by bonding the wet body. However, due to the changes in structure and humidity, the traditional wet body adhesive is not suitable for bonding the wet body, and it is not easy to firmly bond the wet body together. Even if they are bonded together, the connection strength of the joint cannot meet the standard requirements after calcination. Summary of the invention

[0004] In view of the above-mentioned technical problems existing in the prior art, the present disclosure provides an adhesive for biscuit blanks, an adhesive preparation method and a ceramic preparation method. The adhesive is suitable for pasting biscuit blanks together, and after calcination and forming, the pasted parts have a high connection strength.

[0005] An adhesive for biscuit-fired blanks, the adhesive comprising the following components in parts by mass:

[0006] 40-90 parts of calcined clay;

[0007] 0.5-10 parts of clay;

[0008] 0.5-10 parts of calcined kaolin;

[0009] 0.5-10 parts of flux;

[0010] 0.5 to 10 parts of shrinkage stabilizer;

[0011] Thickener 0.5-5 parts;

[0012] 25-35 parts of water.

[0013] In some embodiments, the flux is selected from at least one of the following substances:

[0014] Fluorite, aluminum oxide, and zinc oxide.

[0015] In some embodiments, the shrinkage stabilizer comprises aluminum silicate fibers.

[0016] In some embodiments, the thickening agent comprises methylcellulose and / or xanthan gum.

[0017] In some embodiments, the adhesive specifically includes the following components by weight:

[0018] 45-81 parts of calcined clay;

[0019] 3 to 5 portions of clay;

[0020] 3-4 parts of calcined kaolin;

[0021] 2.5-4 parts of zinc oxide;

[0022] 2-4 parts of calcined aluminum silicate fiber;

[0023] 1.5-2 parts of methylcellulose or xanthan gum;

[0024] 28-30 parts of water.

[0025] A method for preparing an adhesive, for preparing the adhesive as described above, the method comprising:

[0026] The calcined mud, mud, calcined kaolin, flux, shrinkage stabilizer, thickener and water are mixed and processed into an adhesive of a preset fineness.

[0027] In some embodiments, the calcined mud, mud, calcined kaolin, flux, shrinkage stabilizer, thickener and water are mixed and processed into an adhesive with a preset fineness, including:

[0028] Grinding the mixture and water, wherein the mixture comprises 40-90 parts of calcined clay, 0.5-10 parts of clay, 0.5-10 parts of calcined kaolin, 0.5-10 parts of flux, 0.5-10 parts of shrinkage stabilizer and 0.5-5 parts of thickener;

[0029] Filtering the ground material to obtain the material with the preset fineness;

[0030] The material obtained by filtration is dehydrated to obtain the adhesive containing 25 to 35 parts of water.

[0031] A method for preparing ceramics, comprising:

[0032] Using the adhesive as described above, two or more hard bisque-fired blanks are glued together to form a spliced ​​piece;

[0033] The spliced ​​parts are sintered to obtain a finished ceramic product.

[0034] In some embodiments, the method further comprises:

[0035] Before the two or more hard bisque fired blanks are bonded together into a spliced ​​piece by using the adhesive, the hard bisque fired blanks are cut.

[0036] In some embodiments, the method further comprises:

[0037] After two or more hard bisque-fired blanks are bonded together into a spliced ​​piece by using the adhesive, the spliced ​​piece is glazed.

[0038] The adhesive for bisque-fired blanks of the embodiment of the present invention has a unique formula, good operability, soft adhesive, high bonding strength, thin adhesive coating, etc., and is sintered after pasting, with high smoothness at the joint and smooth feel. The ceramic finished product made of the adhesive has been tested for thermal shock resistance by the ceramic testing center, and the thermal shock resistance meets the requirements of the GB / T3532-2009 daily-use porcelain standard.

[0039] The present invention completely changes the 5,000-year history of China's traditional wet-blank pasting process, overcomes the defects of traditional processes, and the products have been tested to have better thermal stability than those produced by traditional processes. It can not only reduce the dependence of enterprises on skilled workers, improve the overall quality of ceramic products, reduce the defective rate, and improve production efficiency, but also reduce raw material loss, save energy and reduce emissions, and benefit environmental protection; and it can create the prerequisites for the mechanized, automated, and standardized production of ceramic products, creating greater economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In the drawings, which are not necessarily drawn to scale, the same reference numerals may describe similar parts in different views. The same reference numerals with letter suffixes or different letter suffixes may represent different instances of similar parts. The accompanying drawings generally illustrate various embodiments by way of example and not limitation, and together with the specification and claims, are used to illustrate the disclosed embodiments. When appropriate, the same reference numerals are used throughout the drawings to refer to the same or similar parts. Such embodiments are illustrative and are not intended to be exhaustive or exclusive embodiments of the present apparatus or method.

[0041] Figure 1 This is a flow chart of a method for preparing an adhesive according to an embodiment of the present invention;

[0042] Figure 2A flow chart of an embodiment of a ceramic preparation method according to an embodiment of the present invention;

[0043] Figure 3 The present invention is a flowchart of another embodiment of the ceramic preparation method of the present invention. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is described in detail below in conjunction with the drawings and specific implementation methods. The embodiments of the present disclosure are further described in detail below in conjunction with the drawings and specific implementation methods, but are not intended to limit the present disclosure.

[0045] The words "first", "second" and similar words used in this disclosure do not indicate any order, quantity or importance, but are only used to distinguish different parts. The words "include" or "comprise" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0046] In the present disclosure, when a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device. When a specific device is described as being connected to other devices, the specific device may be directly connected to the other device without an intermediate device, or may not be directly connected to the other device but have an intermediate device.

[0047] All terms (including technical terms or scientific terms) used in the present disclosure have the same meanings as those understood by ordinary technicians in the field to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, such as general dictionaries, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0048] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.

[0049] The embodiment of the present invention provides an adhesive for bisque fired blanks, which is used to stick bisque fired blanks together. The adhesive includes the following components by weight: 40-90 parts of calcined clay; 0.5-10 parts of clay; 0.5-10 parts of calcined kaolin; 0.5-10 parts of flux; 0.5-10 parts of shrinkage stabilizer; 0.5-5 parts of thickener; and 25-35 parts of water.

[0050] The adhesive of the embodiment of the present invention has good operability, soft glue, high bonding strength, and thin adhesive coating. After sintering, the bonding part not only has high connection strength but also has high smoothness and smooth feel.

[0051] Clay, also known as green material or brick material, is the raw material for producing ceramic green bodies. Its main components include plastic raw materials, barren raw materials and fusible raw materials. Plastic raw materials mainly include clay. Barren raw materials have poor plasticity. Their main function is to form a ceramic skeleton so that the ceramic is not easily deformed during the calcination process. Representative materials include quartz, etc. The main function of fusible raw materials is to reduce the sintering temperature of ceramics. They mainly include potassium feldspar, sodium feldspar, etc. In specific implementation, the clay can be selected from any value between 0.5 and 10 parts, for example, 0.5, 1, 1.5, 2, 3, 5, 7, 9 or 10 parts, etc.

[0052] Calcined clay is also called porcelain clinker. It is a material formed by sintering clay in a calcining furnace to a certain temperature and time to change its physical and chemical properties. In specific implementation, the calcined clay can be selected from any value between 40 and 90 parts, for example, 40 parts, 45 parts, 50 parts, 60 parts, 70 parts, 80 parts, 81 parts, 85.5 parts or 90 parts.

[0053] Calcined kaolin is sintered in a calcining furnace to a certain temperature and time, so that its physical and chemical properties undergo certain changes. The resulting material is called calcined kaolin. In specific implementation, the calcined kaolin can be selected from any value between 0.5 parts and 10 parts, for example, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 5 parts, 6 parts, 7 parts or 10 parts.

[0054] Flux refers to a substance that can reduce the softening, melting or liquefaction temperature of a substance. Fluxes mainly include alkaline fluxes, acidic fluxes and neutral fluxes, wherein alkaline fluxes mainly include calcium oxide, magnesium oxide, etc., acidic fluxes mainly include silicon dioxide, etc., and neutral fluxes mainly include fluorite, aluminum oxide, zinc oxide, etc. In some embodiments, the flux is selected from at least one of the following substances: fluorite, aluminum oxide and zinc oxide. In specific implementation, the flux can be selected from any value between 0.5 parts and 10 parts, for example, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 3 parts, 5 parts, 7 parts, 9 parts or 10 parts, etc.

[0055] The shrinkage stabilizer refers to a material with good thermal shrinkage stability, such as a refractory material with high thermal shrinkage stability. In some embodiments, the shrinkage stabilizer may include aluminum silicate fiber. In specific implementations, the shrinkage stabilizer may be selected from any value between 0.5 and 10 parts, for example, 0.5, 1, 1.5, 2, 3, 4, 6.5, 8 or 10 parts.

[0056] Thickeners, also known as gelling agents, are substances that can increase the viscosity of latex or liquid. In some embodiments, the thickeners may include methylcellulose and / or xanthan gum. In specific implementations, the thickeners may be selected from any value between 0.5 and 5 parts, for example, 0.5, 1, 1.5, 2, 3, 4 or 5 parts.

[0057] It should be noted that the fluxing agents, shrinkage stabilizers and thickeners listed above are only exemplary and should not be construed as being limited to the fluxing agents, shrinkage stabilizers and thickeners listed above. In specific implementations, other types of fluxing agents, shrinkage stabilizers and thickeners may also be used.

[0058] In some embodiments, the adhesive specifically includes the following components by weight: 45-81 parts of calcined clay; 3-5 parts of clay; 3-4 parts of calcined kaolin; 2.5-4 parts of zinc oxide; 2-4 parts of calcined aluminum silicate fiber; 1.5-2 parts of methyl cellulose or xanthan gum; 28-30 parts of water. The adhesive made using this formula not only has excellent performance, but also has easy-to-obtain raw materials and low cost.

[0059] The embodiment of the present invention further provides a method for preparing an adhesive, which is used to prepare the adhesive as described in any of the above embodiments. The method for preparing the adhesive may specifically include the following steps:

[0060] S100, calcined mud, mud, calcined kaolin, flux, shrinkage stabilizer, thickener and water are mixed and processed into an adhesive with a preset fineness.

[0061] That is, calcined mud, mud, calcined kaolin, flux, shrinkage stabilizer, thickener and water are mixed and processed into a paste-like adhesive with a preset fineness.

[0062] Optionally, the preset fineness may be 200 mesh, 120 mesh or other mesh sizes that can meet the bonding requirements of biscuit blanks.

[0063] In the specific implementation, the above materials that meet the preset fineness requirements can be directly purchased, and then mixed with water to form a slurry-like adhesive. Alternatively, the above raw materials with larger particle sizes can be purchased and crushed or ground to the preset fineness.

[0064] Cooperate Figure 1As shown, in some embodiments, step S100, calcined mud, mud, calcined kaolin, flux, shrinkage stabilizer, thickener and water are mixed and processed into an adhesive with a preset fineness, which may specifically include the following steps.

[0065] S110, grinding a mixture with a mass ratio of 1:1 and water, wherein the mixture includes 40-90 parts of calcined clay, 0.5-10 parts of clay, 0.5-10 parts of calcined kaolin, 0.5-10 parts of flux, 0.5-10 parts of shrinkage stabilizer, and 0.5-5 parts of thickener. Optionally, a mixture with a mass ratio of 1:1:2, water, and ball milling particles can be added to a ball mill and ground for 3 to 5 hours, for example.

[0066] It should be noted that the above mass ratio is only exemplary and can be adaptively adjusted according to different grinding equipment.

[0067] S120, filtering the ground material to remove the material with a larger particle size, and obtaining a material with a preset fineness. Optionally, when the preset fineness is 200 mesh, the ground material can be filtered through a 200 mesh sieve to remove the coarse material with a particle size larger than 200 mesh, and obtain a material larger than 200 mesh.

[0068] S130, dehydrating the filtered material to obtain the adhesive containing 25 to 35 parts of water. Optionally, the filtered material can be precipitated to remove the top layer of clear liquid to obtain the bottom layer of slurry-like precipitate, which is the finished adhesive.

[0069] The adhesive is prepared by the processing technology, not only is dust not easily generated during the production process, but the prepared adhesive slurry is fine and delicate, which is beneficial to improving the smoothness of the surface of ceramic products.

[0070] It should be noted that the above processing technology is only exemplary, and in specific implementation, it can only produce an adhesive with a preset fineness and a preset ratio.

[0071] The adhesive and the preparation method of the adhesive according to the embodiment of the present invention are described in detail below in conjunction with specific embodiments.

[0072] Example 1

[0073] An adhesive for bisque fired blanks comprises the following components by weight: 45 parts of calcined clay; 5 parts of clay; 4 parts of calcined kaolin; 2.5 parts of zinc oxide; 4 parts of calcined aluminum silicate fibers; 2 parts of methyl cellulose; and 28 parts of water.

[0074] The adhesive preparation method comprises the following steps:

[0075] A mixture, water and a ball mill in a mass ratio of 1:1:2 are added into a ball mill and ground for 3 hours, wherein the mixture includes 45 parts of calcined mud, 5 parts of mud, 4 parts of calcined kaolin, 2.5 parts of zinc oxide, 4 parts of calcined aluminum silicate fiber and 2 parts of methyl cellulose.

[0076] The ground material is filtered through a 200-mesh sieve to remove the material with larger particle size and obtain the material with a preset fineness.

[0077] The filtered material is precipitated, the clear liquid on the top layer is removed, and the slurry-like precipitate on the bottom layer is obtained as the finished adhesive.

[0078] Example 2

[0079] An adhesive for bisque fired blanks comprises the following components by weight: 81 parts of calcined clay; 3 parts of clay; 3 parts of calcined kaolin; 4 parts of zinc oxide; 2 parts of calcined aluminum silicate fibers; 1.5 parts of methyl cellulose; and 30 parts of water.

[0080] The adhesive preparation method comprises the following steps:

[0081] A mixture, water and a ball mill in a mass ratio of 1:1:2 were added into a ball mill and ground for 4 hours, wherein the mixture included 81 parts of calcined mud, 3 parts of mud, 3 parts of calcined kaolin, 4 parts of zinc oxide, 2 parts of calcined aluminum silicate fiber and 1.5 parts of methyl cellulose.

[0082] The ground material is filtered through a 200-mesh sieve to remove the material with larger particle size and obtain the material with a preset fineness.

[0083] The filtered material is heated and dehydrated at a temperature of 80-100° C. to obtain an adhesive product containing 30 parts of water.

[0084] Example 3

[0085] An adhesive for bisque fired blanks comprises the following components by weight: 54 parts of calcined clay; 4 parts of clay; 3.5 parts of calcined kaolin; 3.5 parts of zinc oxide; 3 parts of calcined aluminum silicate fiber; 2 parts of xanthan gum; and 30 parts of water.

[0086] The adhesive preparation method comprises the following steps:

[0087] A mixture, water and a ball mill in a mass ratio of 1:1:2 are added into a ball mill and ground for 5 hours, wherein the mixture includes 54 parts of calcined mud; 4 parts of mud; 3.5 parts of calcined kaolin; 3.5 parts of zinc oxide; 3 parts of calcined aluminum silicate fiber; and 2 parts of xanthan gum.

[0088] The ground material is filtered through a 200-mesh sieve to remove the material with larger particle size and obtain the material with a preset fineness.

[0089] The filtered material is precipitated, the clear liquid on the top layer is removed, and the slurry-like precipitate on the bottom layer is obtained as the finished adhesive.

[0090] Example 4

[0091] An adhesive for bisque fired blanks comprises the following components by weight: 90 parts of calcined clay; 0.5 parts of clay; 0.5 parts of calcined kaolin; 6 parts of alumina; 6 parts of calcined aluminum silicate fiber; 1 part of xanthan gum; and 35 parts of water.

[0092] The adhesive preparation method comprises the following steps:

[0093] A mixture, water and a ball mill in a mass ratio of 1:1:2 are added into a ball mill and ground for 3.5 hours, wherein the mixture includes 90 parts of calcined mud; 0.5 parts of mud; 0.5 parts of calcined kaolin; 6 parts of alumina; 6 parts of calcined aluminum silicate fiber; and 1 part of xanthan gum.

[0094] The ground material is filtered through a 120-mesh sieve to remove the material with larger particle size and obtain the material with preset fineness.

[0095] The filtered material is precipitated, the clear liquid on the top layer is removed, and the slurry-like precipitate on the bottom layer is obtained as the finished adhesive.

[0096] Example 5

[0097] An adhesive for bisque fired blanks comprises the following components by weight: 40 parts of calcined clay; 10 parts of clay; 10 parts of calcined kaolin; 2 parts of alumina; 10 parts of calcined aluminum silicate fibers; 0.5 parts of methyl cellulose; and 25 parts of water.

[0098] The adhesive preparation method comprises the following steps:

[0099] A mixture, water and a ball mill in a mass ratio of 1:1:2 are added into a ball mill and ground for 5 hours, wherein the mixture includes 40 parts of calcined mud; 10 parts of mud; 10 parts of calcined kaolin; 2 parts of alumina; 10 parts of calcined aluminum silicate fiber; and 0.5 parts of methyl cellulose.

[0100] The ground material is filtered through a 200-mesh sieve to remove the material with larger particle size and obtain the material with a preset fineness.

[0101] The filtered material is heated and dehydrated at 80° C. to 100° C. to obtain a finished adhesive product.

[0102] The adhesive for bisque-fired blanks of the embodiment of the present invention has a unique formula, good operability, soft glue, high bonding strength, thin adhesive coating, etc., and is sintered after pasting, with high smoothness at the joint and smooth feel. The ceramic products made of the adhesive of any of the above embodiments are tested for thermal shock resistance by the ceramic testing center, and the thermal shock resistance meets the requirements of the GB / T3532-2009 daily-use porcelain standard.

[0103] The present invention completely changes the 5,000-year history of China's traditional wet-blank pasting process, overcomes the defects of traditional processes, and the products have been tested to have better thermal stability than those produced by traditional processes. It can not only reduce the dependence of enterprises on skilled workers, improve the overall quality of ceramic products, reduce the defective rate, and improve production efficiency, but also reduce raw material loss, save energy and reduce emissions, and benefit environmental protection; and it can create the prerequisites for the mechanized, automated, and standardized production of ceramic products, creating greater economic and social benefits.

[0104] See also Figure 2 As shown, an embodiment of the present invention further provides a ceramic preparation method, which may specifically include the following steps.

[0105] S210, using the adhesive as described in any of the above embodiments to glue two or more hard bisque-fired blanks into a spliced ​​part.

[0106] S220, sintering the assembled parts to obtain a finished ceramic product.

[0107] The ceramic preparation method of the embodiment of the present invention uses an adhesive to stick hard biscuit blanks into spliced ​​parts, and then sinter the spliced ​​parts to obtain finished ceramic products. The hard biscuit blanks have a certain mechanical strength, are not easy to deform, and are not easy to have pressing marks, which is beneficial to improving the authenticity rate, reducing manual operation steps, and improving the product quality of ceramic products.

[0108] The specific steps and principles of the ceramic preparation method according to the embodiment of the present invention are described in detail below in conjunction with specific embodiments.

[0109] See also Figure 3 As shown, the ceramic preparation method according to the embodiment of the present invention may specifically include the following steps.

[0110] S301, making a clay blank and drying the clay blank.

[0111] Optionally, clay blanks may be made according to the main form of the finished product object. Taking the ceramic finished product as a pot as an example, clay blanks such as a pot body, a pot spout and a pot handle may be prepared.

[0112] Optionally, after the clay is prepared, the clay can be placed in a gypsum mold and initially shaped using the gypsum mold, and the initially shaped clay can be placed in an upper roller for rolling, or placed in a high-pressure grouting machine for extrusion, thereby achieving the purpose of making clay blanks according to the shape of the finished object.

[0113] Optionally, after the clay material is prepared and bent, a throwing machine can be used to throw the clay material into a clay blank.

[0114] Optionally, after the mud blank is made, the water in the mud blank can be evaporated by air-drying or drying. Optionally, the mud blank is placed in a mud blank drying device, for example, and dried at a specific temperature and humidity.

[0115] S302, biscuit-firing the dried clay blank to obtain a hard biscuit-fired blank.

[0116] Optionally, an electric furnace or a gas furnace can be used to bisque-fire the clay blank, specifically an electric kiln or a gas kiln. The bisque-fire temperature can be determined according to the ratio between the components of the clay blank, so as to bisque-fire the clay blank in a targeted manner. The components of the above-mentioned clay blank can be composed of one or more oxides, such as aluminum oxide, silicon oxide, potassium oxide, and sodium oxide. In the case where the components of the clay blank include aluminum oxide, silicon oxide, potassium oxide, and sodium oxide, the corresponding bisque-fire temperature can be determined according to the ratio of the components between aluminum oxide, silicon oxide, potassium oxide, and sodium oxide. For example, when the ratio of aluminum oxide, silicon oxide, potassium oxide, and sodium oxide is 1:2:3:1, the bisque-fire temperature can range from 760 degrees Celsius to 780 degrees Celsius; when the ratio of aluminum oxide, silicon oxide, potassium oxide, and sodium oxide is 1:2:2:1, the bisque-fire temperature can range from 810 degrees Celsius to 820 degrees Celsius.

[0117] It should be noted that the present invention does not specifically limit the ratio of the various components of the clay blank, and the bisque firing temperature can be adaptively adjusted according to the ratio parameters of the various components of the clay blank.

[0118] Optionally, by controlling the biscuit firing time of the clay blank, a hard biscuit blank with a Mohs hardness between 3.5 and 5.2 can be obtained. The hard biscuit blank within the Mohs hardness range has appropriate hardness and toughness, is suitable for cutting and assembly, and is not prone to deformation, pressing marks, or breakage.

[0119] S303, cutting the hard biscuit blank.

[0120] Optionally, after the biscuit firing of the hard biscuit blank is completed, the hard biscuit blank may be placed in a kiln for about 8 hours to allow the hard biscuit blank to cool.

[0121] Optionally, after the hard sintered blank is cooled, the hard sintered blank may be cut by, for example, a CNC lathe using a cemented carbide tool.

[0122] S304, using the adhesive to glue two or more hard bisque-fired blanks that have been cut to form a spliced ​​piece.

[0123] Optionally, after the cutting process is completed, the hard bisque-fired blanks that have been cut can be stably pasted together according to the pre-designed image of the finished ceramic product to form a spliced ​​piece, which actually already has the overall shape of the finished ceramic product.

[0124] S305, glazing the spliced ​​parts obtained by pasting.

[0125] Optionally, before glazing the spliced ​​piece obtained by pasting, the pasting position can be corrected using a trimming tool or manually to ensure that the surface of the spliced ​​piece is smooth and flat.

[0126] S306, sintering the glazed assembly to obtain a finished ceramic product.

[0127] In addition, although exemplary embodiments have been described herein, the scope includes any and all embodiments based on the present disclosure with equivalent elements, modifications, omissions, combinations (e.g., various embodiments intersecting schemes), adaptations or changes. The elements in the claims will be interpreted broadly based on the language adopted in the claims, and are not limited to the examples described in this specification or during the implementation of this application, and the examples will be interpreted as non-exclusive. Therefore, this specification and examples are intended to be considered as examples only, and the true scope and spirit are indicated by the following claims and the full scope of their equivalents.

[0128] The above description is intended to be illustrative rather than restrictive. For example, the above examples (or one or more of them) can be used in combination with each other. For example, a person of ordinary skill in the art can use other embodiments when reading the above description. In addition, in the above-mentioned specific embodiments, various features can be grouped together to simplify the present disclosure. This should not be interpreted as an intention that a disclosed feature that is not required to be protected is necessary for any claim. On the contrary, the subject matter of the present disclosure may be less than all the features of a specific disclosed embodiment. Thus, the following claims are incorporated into the specific embodiments as examples or embodiments, wherein each claim is independently used as a separate embodiment, and it is considered that these embodiments can be combined with each other in various combinations or arrangements. The scope of the present disclosure should be determined with reference to the attached claims and the full scope of equivalent forms granted by these claims.

[0129] The above embodiments are only exemplary embodiments of the present disclosure and are not intended to limit the present disclosure. The protection scope of the present disclosure is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present disclosure within the essence and protection scope of the present disclosure, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present disclosure.

Claims

1. An adhesive for biscuit-fired blanks, characterized in that: The adhesive comprises the following components in parts by mass: 40-90 parts of calcined clay; 0.5-10 parts of clay; 0.5-10 parts of calcined kaolin; 0.5-10 parts of flux; 0.5 to 10 parts of shrinkage stabilizer; Thickener 0.5-5 parts; 25-35 parts water; Wherein, the flux is selected from one of fluorite, aluminum oxide and zinc oxide, and the main components of the mud include plastic raw materials, barren raw materials and fusible raw materials, the plastic raw materials include clay, the barren raw materials include quartz, and the fusible raw materials include potassium feldspar or sodium feldspar.

2. The adhesive according to claim 1, characterized in that The shrinkage stabilizer includes aluminum silicate fibers.

3. The adhesive according to claim 1, characterized in that The thickener includes methylcellulose and / or xanthan gum.

4. The adhesive according to claim 1, characterized in that The adhesive specifically comprises the following components in parts by mass: 45-81 parts of calcined clay; 3 to 5 portions of clay; 3-4 parts of calcined kaolin; 2.5-4 parts of zinc oxide; 2-4 parts of calcined aluminum silicate fiber; 1.5-2 parts of methylcellulose or xanthan gum; 28-30 parts of water.

5. A method for preparing an adhesive, characterized in that: For preparing the adhesive according to any one of claims 1 to 4, the method comprises: The calcined mud, mud, calcined kaolin, flux, shrinkage stabilizer, thickener and water are mixed and processed into an adhesive of a preset fineness.

6. The method according to claim 5, characterized in that The calcined mud, mud, calcined kaolin, flux, shrinkage stabilizer, thickener and water are mixed and processed into an adhesive with a preset fineness, including: Grinding the mixture and water, wherein the mixture comprises 40-90 parts of calcined clay, 0.5-10 parts of clay, 0.5-10 parts of calcined kaolin, 0.5-10 parts of flux, 0.5-10 parts of shrinkage stabilizer and 0.5-5 parts of thickener; Filtering the ground material to obtain the material with the preset fineness; The material obtained by filtration is dehydrated to obtain the adhesive containing 25 to 35 parts of water.

7. A method for preparing ceramics, characterized in that: include: Using the adhesive as claimed in any one of claims 1 to 4 to glue two or more hard bisque-fired blanks into a spliced ​​part; The spliced ​​parts are sintered to obtain a finished ceramic product.

8. The method according to claim 7, characterized in that The method further comprises: Before the two or more hard bisque fired blanks are bonded together into a spliced ​​piece by using the adhesive, the hard bisque fired blanks are cut.