Low-temperature solid-phase synthesis of L / B-site co-doped yttrium aluminum garnet powder

Through the low-temperature solid-phase synthesis method, ball milling and sand milling are used to process the raw materials, and combined with absolute ethanol and polymethacrylic acid amine, the high-purity and impurity-free preparation of yttrium aluminum garnet powder is achieved, solving the existing technical problems. In order to solve the problems of uneven distribution of medium components and high production costs, high-purity, L/B-site co-doped YAG powder with controllable doping ions was obtained.

CN116655366BActive Publication Date: 2024-10-01INNER MONGOLIA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310408162.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-01
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

It is difficult to effectively prepare high-purity, impurity-free yttrium aluminum garnet powder with the existing technology, especially in the case of L/B site co-doping. There are problems such as uneven component distribution, difficulty in accurately controlling doping elements, and high production costs. question.

Method used

Adopting low-temperature solid-phase synthesis method, the raw materials are processed by ball milling and sand grinding to obtain ultra-fine powder, which is then sintered at 1100-1300°C. Absolute ethanol and polymethacrylic acid amine are combined as dispersants to control the sintering temperature and The heating rate enables controllable occupancy of doping ions in the YAG lattice.

Benefits of technology

It achieves composition uniformity, high purity, and controllable doping ion occupancy of yttrium aluminum garnet powder, reduces sintering temperature and production costs, avoids the introduction of impurities, and obtains high-purity, impurity-free L/B sites. Co-doped YAG powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116655366B_ABST
    Figure CN116655366B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-temperature solid-phase synthesis method of L / B co-doped yttrium aluminum garnet powder. First, the raw materials are processed, and after ball milling and sand milling, all the raw materials are refined to nanometer level to create conditions for subsequent low-temperature sintering. In the sintering process of YAG powder, a combination of ball milling and grinding is adopted to improve the fineness and uniformity of the powder, promote solid-phase reaction, and because the sintering temperature is low and the heating rate is low, the diffusion time of the doped ions in the YAG matrix is ​​prolonged, thereby obtaining sufficient solid solution and realizing controllable position of the doped ions in the YAG lattice. The obtained (YAG) 1‑x L x )3(Al 1‑y B y )5O 12 (0
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a compound preparation technology, in particular to a large-scale preparation technology of oxide ceramic powder doped with multiple elements. Background Art

[0002] Yttrium aluminum garnet (Y3Al5O 12 As a man-made compound, YAG has stable chemical properties, excellent optical properties and high-temperature mechanical properties. It is widely used in the fields of phosphors, laser media and thermal barrier coatings.

[0003] YAG belongs to the cubic crystal system, and its general chemical formula is L3B2(AO4)3 (L, A, and B represent three lattice positions, respectively). 3+ In the 8 O 2- Coordinated dodecahedral L lattice site, Al 3+ In 6 O 2- The coordinated octahedral B site and 4 O 2- Coordinated tetrahedral A lattice, therefore, the YAG unit cell can be regarded as a connection network of dodecahedron, octahedron and tetrahedron, with very good structural compatibility, and it is easy to introduce cations with a larger ionic radius for doping replacement, thereby changing the physical properties of the material: the introduction of Ce 3+ 、Eu 3+ Doping can enhance the fluorescence performance of YAG materials. 3+ , Yb 3+ Doping can improve the laser performance of YAG transparent ceramics. 3+ , Fe 3+ Doping can reduce the thermal conductivity of YAG ceramics and increase its thermal expansion coefficient.

[0004] For example, in the early 1970s, researchers discovered that Ce-doped YAG can emit strong yellow fluorescence when excited by visible light, and then developed YAG phosphors doped with Dy, Eu, and Tb. In 1995, Krosaki of Japan produced high-quality Nd:YAG transparent ceramics and achieved effective laser oscillation for the first time. Currently, the United States has developed Nd:YAG solid lasers with a laser output power of up to 67kW. In 1997, Padture et al. studied Y3Al x Fe 5-x O 12 When the thermal conductivity of ceramics (x=0, 0.7, 1.4, 5.0) was investigated, it was found that the high-temperature thermal conductivity of some garnets was as low as 2.4 W / m·K, which suggested the possibility of using YAG materials as thermal barrier coatings.

[0005] However, the position of dopant ions in the YAG lattice has a crucial influence on the material properties. Taking the thermophysical properties as an example, when Er 3+ Y substituted for the L site of YAG dodecahedron 3+ When Y2ErAl5O with low thermal conductivity is obtained 12 Ceramic (1.8W / m·K, 1000℃), but its thermal expansion coefficient has not improved, and is still 8.63×10 at 1157℃. -6 K -1 When Yb 3+ Al replaces the B site of YAG octahedron 3+ When the thermal conductivity of the material at room temperature is lower than that of pure YAG, it is about 2.11W / m·K, and the thermal expansion coefficient is significantly increased, exceeding 10×10 at 800℃. -6 K -1 It can be seen that the lattice occupancy of the doped ions has a significant effect on the thermal physical properties of YAG. Both L-site doping with dodecahedrons and B-site octahedrons can reduce the thermal conductivity of YAG to varying degrees, while B-site octahedrons are more likely to increase the thermal expansion coefficient of the material. Therefore, co-doping at L and B sites is the best solution to effectively improve the physical properties of yttrium aluminum garnet materials.

[0006] On the other hand, since YAG can be regarded as a composite oxide of yttrium oxide and aluminum oxide, the phase region of YAG is a line, that is, each element needs to meet a precise stoichiometric ratio to form, and there are also strict requirements on the synthesis temperature. Therefore, the selection of the preparation method and how to control the ratio of each element are crucial to the successful synthesis of L / B co-doped YAG.

[0007] At present, the methods for preparing yttrium aluminum garnet powder materials at home and abroad mainly include high-temperature solid phase method, liquid phase precipitation method, hydrothermal synthesis method and sol-gel method, etc.

[0008] For example, the powder of the liquid phase precipitation method is easy to agglomerate, and because different cations have different sensitivities to pH values, it is easy to produce sequential precipitation, resulting in uneven distribution of powder components; the hydrothermal synthesis method requires reactions under high temperature and high pressure conditions, has high requirements for equipment and environment, and has low yield and poor purity, making it difficult to produce on a large scale; the sol-gel method can obtain YAG powder at a relatively low temperature, but it often requires the addition of chelating agents such as citric acid and triethanolamine, which will inevitably introduce impurity elements such as N or C, affecting the purity of the final YAG product, and the drying and roasting processes may lead to the formation of particle agglomerations, making it difficult to form evenly dispersed YAG powder; YAG synthesized by the high-temperature solid phase method often has a calcination temperature above 1600°C, resulting in large powder particles, uneven chemical composition, and the easy appearance of YAM (Y4Al2O9) and YAP (YAlO3) impurities, as well as high energy consumption and cost.

[0009] Moreover, the YAG powder materials prepared by the above method mainly focus on the study of L-site doping, because the B-site space is smaller than the L-site, and improper doping is easy to disturb the phase formation and produce impurities. Therefore, there is still a large gap in the preparation of L / B-site co-doped YAG powder materials.

[0010] Therefore, the development of an L / B co-doped YAG powder with uniform composition distribution, precise and controllable doping elements and low production cost and its preparation method are of great significance for the research and application of YAG materials. Summary of the invention

[0011] In view of the above problems, the present invention aims to provide a low-temperature solid phase synthesis method that can realize large-scale preparation of high-purity, impurity-free yttrium aluminum garnet powder. The method is particularly suitable for preparing L / B co-doped yttrium aluminum garnet powder.

[0012] The technical solution of the present invention is as follows.

[0013] A low-temperature solid-phase synthesis method of L / B-site co-doped yttrium aluminum garnet powder comprises the following steps:

[0014] S1, Y2O3, L-doped element compound, Al(OH)3 and B-doped element compound are used as raw materials and ball milled respectively;

[0015] S2, further sand-milling the raw materials after ball milling in S1, and drying to obtain ultrafine powders of the four raw materials;

[0016] S3, mixing and ball-milling the ultrafine powders of the four raw materials obtained in S2 according to the ratio of each element in the product, and drying, grinding and sieving after completion;

[0017] S4, sintering the sieve material in S3 at 1100-1300° C. to obtain L / B site co-doped yttrium aluminum garnet powder.

[0018] The scheme disclosed by the present invention first processes the raw materials to create conditions for low-temperature sintering; then the processed raw materials are mixed to sinter the YAG powder into phases, and the position of the doped ions in the YAG lattice is controllable at a relatively low temperature and heating rate.

[0019] Preferably, the L-site doping element is Er, Gd, Sc, Ce, Yb or Nd, and the B-site doping element is Fe, Mg, Ti, Ca or Mn.

[0020] Further preferably, the compound of the L-site doping element is Er2O3, Gd2O3, Sc2O3, CeO2, Yb2O3 or Nd2O3, and the raw material of the B-site doping element is Fe2O3, MgO, TiO2, CaCO3 or MnCO3.

[0021] Preferably, water is used as the dispersant in the ball milling in S1.

[0022] Specifically, when ball milling rare earth oxides, the solid content is less than 40%, when ball milling metal oxides, the solid content is less than 30%, and when ball milling hydroxides and carbonates, the solid content is less than 20%.

[0023] Preferably, for the sand milling in S2, first sand mill at 2300 rpm for 1 h, then sand mill at 2500 rpm for 1 h, and finally sand mill at 2700 rpm for 1 h. Through the comparison of different rotation speeds and times, it is found that under this condition, the obtained material is finer and the sand milling treatment time is also appropriate, which is a preferred sand milling parameter with the characteristics of economy and high efficiency.

[0024] Further preferably, during the sand milling in S2, poly(meth)acrylamide is added as the dispersant. And for different raw materials, the addition amount of the dispersant is different.

[0025] Specifically, for rare earth oxide raw materials, the addition amount of the dispersant does not exceed 4 wt‰; for metal oxide raw materials, the addition amount of the dispersant does not exceed 1 wt%; for hydroxide and carbonate raw materials, the addition amount of the dispersant does not exceed 2 wt%.

[0026] Preferably, in S3, ultra-fine powders of four raw materials are mixed according to (Y 1-x L x )3(Al 1-y B y )5O 12 (0 < x < 1; 0 < y < 1).

[0027] Preferably, during the mixed ball milling in S3, absolute ethanol is added, and the mass ratio of the raw material to absolute ethanol is 1:2.

[0028] Preferably, for the drying in S3, the material is placed in a beaker, sealed with a film with air holes, and dried at a constant temperature of 70 - 90 °C. For example, the beaker mouth can be sealed with a film, and several small holes can be pricked on the film with a knife. Preferably, for the sieving in S3, it is sieved through a 80 - 200 mesh sieve.

[0029] Preferably, for the sintering in S4, heat up to 1000 °C at a rate of 5 °C / min, then heat up to 1100 - 1300 °C at a rate of 2 °C / min and hold for 3 - 5 h, and finally cool down at a rate of 100 °C / h.

[0030] In the solution disclosed by the present invention, the raw materials are first processed and ground multiple times. The sand grinding process is one of the prominent features of the present invention, which refines all raw materials to the nanoscale, creating conditions for subsequent low-temperature sintering. During the processing, except for the raw materials and the dispersant, there are no other substances, and the dispersant polyacrylamide can be removed by calcination without washing and without generating waste liquid, which is environmentally friendly. Water is easy to evaporate and anhydrous ethanol is easy to volatilize, and no impurities will remain. Therefore, the obtained yttrium aluminum garnet ceramic powder has high purity and no impurity phase.

[0031] During the phase formation process of YAG powder sintering, a combination of ball milling and grinding and sieving is adopted to achieve fine particle size and uniformity of the powder; hydroxides or carbonates (Al(OH)3, MnCO3, CaCO3) with higher reaction activity are selected to replace the oxide raw materials in the traditional preparation method, which can promote the solid-phase reaction, and there is no loss of other substances during the reaction process. Just according to the calculated raw material ratio, a product with an accurate chemical stoichiometric ratio can be obtained; by reducing the heating rate of the sintering temperature and optimizing the sintering process, the diffusion time of the doped ions in the YAG matrix is extended, so as to obtain sufficient solid solution and realize the controllable occupation of the doped ions in the YAG lattice.

[0032] According to the technical solution of the present invention, there is no composition segregation or loss during the powder processing and solid-phase synthesis process, no impurity is introduced, and the obtained (Y 1-x L x )3(Al 1-y B y )5O 12 (0 < x < 1; 0 < y < 1) powder is a single garnet structure, having the advantages of high purity, uniform composition, accurate chemical stoichiometry, and controllable occupation of doped ions.

[0033] The sand grinding technology introduced in the present invention is a physical method for preparing ultrafine powder. It mainly crushes the powder through the ball milling medium during high-speed operation. This method is simple to operate and easy to control, which can not only meet the high-quality requirements of small particle size, uniform distribution, and good sphericity of the material, but also meet the industrialization requirements of high efficiency, low loss, and low production process cost of the equipment. Specifically in the present invention, after the raw material powder is sand ground, the particle size is uniform and small, with a high specific surface area and high reaction activity, and it is easy to realize the low-temperature phase formation of yttrium aluminum garnet powder during the solid-phase reaction.

[0034] In the present invention, after the material is ball milled, secondary grinding and sieving are carried out, which is not only beneficial to the refinement and homogenization of the powder particle size, further reducing the solid-phase synthesis reaction temperature, but also improving the composition uniformity of the mixed powder, and obtaining a uniformly composed L / B-site co-doped YAG powder.

[0035] Finally, compared with the traditional high-temperature solid-phase reaction of yttrium aluminum garnet powder, the sintering temperature of the present invention is greatly reduced, and the maximum temperature is only 1300°C. The traditional method requires high-temperature sintering above 1600°C to obtain it, and the heating rate is very fast, about 10-20°C / min, which is prone to coarse powder particles and uneven distribution of components. In the present invention, by reducing the heating rate of the sintering temperature, especially the heating rate in the high-temperature stage above 1000°C, the reaction diffusion time can be extended, the doping ions can be fully dissolved in the YAG matrix, and the L / B co-doped YAG powder with controllable lattice occupancy can be obtained, and the production cost is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The flowchart of the low-temperature solid phase synthesis method of the L / B-site co-doped yttrium aluminum garnet powder in Example 1;

[0037] Figure 2 The XRD pattern of the L / B co-doped yttrium aluminum garnet powder obtained in Example 1-5;

[0038] Figure 3 is a SEM image of the L / B-site co-doped yttrium aluminum garnet powder obtained in Example 1;

[0039] Figure 4 This is the EDS image of the L / B co-doped yttrium aluminum garnet powder obtained in Example 1. DETAILED DESCRIPTION

[0040] In order to better explain the present invention, the present invention is explained and illustrated through the following specific implementation modes.

[0041] Example 1

[0042] according to Figure 1 The process described herein is used to prepare L / B co-doped yttrium aluminum garnet powder (Y 0.4 Er 0.6 )3(Al 0.8 Fe 0.2 )5O 12 , the specific steps are as follows.

[0043] S1, place Y2O3, Er2O3, Al(OH)3, Fe2O3 powders with chemical purity ≥99.99% in polyurethane ball mills, and add deionized water as a dispersant. Among them, the mass ratio of Y2O3 powder and Er2O3 powder to water is 1:1.5; the mass ratio of Al(OH)3 powder to water is 1:4; the mass ratio of Fe2O3 powder to water is 3:7. Place the polyurethane ball mill on the jar mill and mill at a speed of 150r / min for 24 hours to reach the sand mill feed particle size requirement as the ball milling end point to prevent coarse particles from clogging the pipeline.

[0044] S2, after the ball milling is completed, the slurry obtained by ball milling is poured into a sand mill, and each raw material is ground for 1 hour at a rotation speed of 2300r / min, 2500r / min and 2700r / min, and at the same time, polymethyl methacrylate dispersant is added dropwise in proportion. Among them, 4wt‰ dispersant is added to Y2O3 powder and Er2O3 powder; 2wt% dispersant is added to Al(OH)3 powder; 1wt% dispersant is added to Fe2O3 powder. After the sand milling is completed, the slurry is poured into a stainless steel tray, and then taken to an oven for drying at 90℃ for 12 hours to obtain ultrafine raw material powder with uniform particle size.

[0045] S3, mix the ultrafine raw material powders of Y2O3, Er2O3, Al(OH)3, and Fe2O3 in a molar ratio of 6:9:40:5 and place them in a nylon ball mill, add anhydrous ethanol as a dispersant, and the mass ratio of dispersant to material is 2:1. Place the nylon ball mill in a planetary ball mill for 24 hours. After the ball milling is completed, pour the material into a beaker, seal the beaker mouth with a film, poke a few small holes with a knife, and put it into an electric constant temperature blast drying oven for 12 hours. The drying oven temperature is 80°C. Grind the dried powder and then sieve it with an 80-mesh sieve.

[0046] S4, pour the sieved powder into a crucible and place it in a box-type resistance furnace for sintering. The sintering temperature is 1300°C, the holding time is 3 hours, and the specific heating program is 5°C / min below 1000°C and 2°C / min above 1000°C. After the holding is completed, the temperature is lowered at a rate of 100°C / h.

[0047] The obtained L / B co-doped yttrium aluminum garnet powder (Y 0.4 Er 0.6 )3(Al 0.8 Fe 0.2 )5O 12 The XRD pattern of Figure 2 As shown, it can be seen that the XRD diffraction pattern of the obtained powder shows a single garnet structure without impurity phase, indicating that Er and Fe are completely dissolved in the YAG lattice.

[0048] The obtained L / B co-doped yttrium aluminum garnet powder (Y 0.4 Er 0.6 )3(Al 0.8 Fe 0.2 )5O 12 The SEM and EDS images are as follows Figure 3-4The atomic percentages of Y, Er, Al, Fe, and O are 6.06%, 9.07%, 20.14%, 4.81%, and 59.92%, respectively, which are close to the atomic ratio of Y, Er, Al, Fe, and O in the powder (6:9:20:5:60). 0.4 Er 0.6 )3(Al 0.8 Fe 0.2 )5O 12 The powder composition is uniform and has a precise stoichiometric ratio.

[0049] Embodiment 2-10

[0050] By replacing different L and B doping elements and raw material ratios, yttrium aluminum garnet powders doped with different L and B elements were prepared according to the same preparation method as in Example 1, as shown in the following table. The raw material ratio is the molar ratio of the four raw materials of Y2O3, L doping raw material, Al(OH)3, and B doping raw material.

[0051]

[0052] Among them, the XRD diffraction patterns of Examples 2-5 are as follows: Figure 2 As shown, it can be determined that the obtained materials are all single garnet structures without impurities.

Claims

1. A low-temperature solid phase synthesis method for L / B co-doped yttrium aluminum garnet powder, characterized in that: The synthesis method comprises the following steps: S1, using Y2O3, a compound of an L-position doping element, Al(OH)3 and a compound of a B-position doping element as raw materials, respectively subjecting them to ball milling; the L-position doping element is Sc, the compound of the L-position doping element is Sc2O3; the B-position doping element is Mn, the compound of the B-position doping element is MnCO3; S2, sand-milling the raw materials after ball milling in S1, and drying to obtain ultrafine powders of the four raw materials; the sand-milling is first sand-milled at 2300 rpm for 1 hour, then sand-milled at 2500 rpm for 1 hour, and finally sand-milled at 2700 rpm for 1 hour; S3, mixing and ball-milling the ultrafine powders of the four raw materials obtained in S2 according to the ratio of each element in the product, and drying and grinding and sieving after completion; S4, sintering the sieve material in S3 at 1100-1300° C. to obtain the L / B-site co-doped yttrium aluminum garnet powder; The sintering is performed by heating the temperature to 1000°C at 5°C / min, then heating the temperature to 1100-1300°C at 2°C / min and keeping the temperature for 3-5h, and finally cooling the temperature at 100°C / h; The L / B-site co-doped yttrium aluminum garnet powder has a single garnet structure.

2. The low-temperature solid phase synthesis method of L / B co-doped yttrium aluminum garnet powder according to claim 1, characterized in that: The ball milling in S1 uses water as a dispersant, wherein the solid content of the rare earth oxide during the ball milling is less than 40%, and the solid content of the hydroxide and carbonate during the ball milling is less than 20%.

3. The low-temperature solid phase synthesis method of L / B co-doped yttrium aluminum garnet powder according to claim 1, characterized in that: During the sand grinding described in S2, polymethacrylamide is added as a dispersant, wherein for rare earth oxides, the amount of the dispersant added does not exceed 4wt‰, and for hydroxides and carbonates, the amount of the dispersant added does not exceed 2wt%.

4. The low-temperature solid phase synthesis method of L / B co-doped yttrium aluminum garnet powder according to claim 1, characterized in that: In S3, according to (Y 1-x Sc x )3(Al 1-y Mn y )5O 12 (0 < x < 1; 0 < y < 1), mix the ultrafine powders of the four raw materials. Add absolute ethanol during the mixing and ball milling, and the mass ratio of the mixed ultrafine powder to the absolute ethanol is 1:

2.

5. The low-temperature solid phase synthesis method of L / B co-doped yttrium aluminum garnet powder according to claim 1, characterized in that: In S3, the drying is to place the material in a beaker, seal it with a film with air permeable holes, and dry it at a constant temperature of 70-90°C.

6. The low-temperature solid phase synthesis method of L / B co-doped yttrium aluminum garnet powder according to claim 1, characterized in that: In S3, the screening is through a 80-200 mesh sieve.