Substrate surface hydrophilic treatment method and substrate with hydrophilic modified surface

By covering and cross-linking hydrophilic polymers on the surface of the substrate to form a chemically bonded hydrophilic modified layer, the problem of insufficient durability of hydrophilic treatment on the substrate surface in the existing technology is solved, and a more durable and washable hydrophilic membrane is achieved. water performance.

CN116655987BActive Publication Date: 2024-10-25WIN Z TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210356791.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-02-21
Filing Date
2022-03-31
Publication Date
2024-10-25
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

The hydrophilicity treatment method of the substrate surface in the existing technology has insufficient durability and cannot maintain the hydrophilicity for a long time. In particular, the hydrophilicity imparted by plasma technology is prone to rapid decline in a short period of time.

Method used

A hydrophilic polymer is used to cover the surface of a substrate with active groups, and a chemically bonded hydrophilic modified layer is formed through a cross-linking reaction. The hydrophilic polymer contains units derived from N-hydroxymethylacrylamide and derived from For the olefin unit substituted by a hydrophilic group, the cross-linking reaction temperature is 80 to 120°C and the time is 0.5 to 15 hours.

Benefits of technology

It significantly improves the hydrophilicity of the substrate surface, is more durable and washable than existing modification technologies, and can maintain good hydrophilic properties in different applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116655987B_ABST
    Figure CN116655987B_ABST
Patent Text Reader

Abstract

A method for hydrophilic treatment of a substrate surface comprises: coating a hydrophilic polymer on a substrate surface having an active group; and causing the hydrophilic polymer to undergo a cross-linking reaction with the active group to obtain a hydrophilic substrate surface; wherein the hydrophilic polymer comprises a unit derived from N-hydroxymethyl acrylamide and a unit derived from an olefin substituted with a hydrophilic group. The present invention further provides a substrate prepared by the method as described above. The method of the present invention can effectively improve the hydrophilicity of the surface, and is more durable and water-resistant than existing modification technologies, and has application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a substrate surface treatment method, in particular to a substrate surface hydrophilic treatment method and a substrate with a hydrophilic modified surface. Background Art

[0002] Surface treatment is a very important process project. Its advantage is that it can further obtain certain properties that the substrate does not possess without changing the essence of the substrate. Therefore, it is widely used in micro-electromechanical, optoelectronics, chemistry, biochemistry, medical materials and other fields.

[0003] Regarding the hydrophilic treatment of substrates, it is often used for hydrophobic materials or substrates with limited affinity for polar liquids (such as glass, plastic, silicon chips, etc.), in order to meet the requirements of wetting, self-cleaning, anti-fouling, anti-static, biocompatibility, etc., and plasma technology is the most common. However, the hydrophilicity imparted by plasma technology tends to decline rapidly in a short period of time and cannot last long.

[0004] In view of this, it is necessary to propose a substrate surface hydrophilic treatment method that is more durable than the prior art to solve the problems existing in the above-mentioned known technologies. Summary of the invention

[0005] To solve the above problems, the present invention provides a method for hydrophilic treatment of a substrate surface, comprising: coating a hydrophilic polymer on a substrate surface having an active group; and causing the hydrophilic polymer to undergo a cross-linking reaction with the active group to obtain a substrate surface having hydrophilicity; wherein the hydrophilic polymer comprises a unit derived from N-hydroxymethyl acrylamide and a unit derived from an olefin substituted with a hydrophilic group.

[0006] In one embodiment of the present invention, the substrate surface having active groups is formed by an activation treatment; in one example, the activation treatment is a plasma treatment, and the plasma gas is oxygen or air.

[0007] In one embodiment of the present invention, the reactive group is a hydroxyl group.

[0008] In one embodiment of the present invention, the material of the substrate is selected from the group consisting of copper foil, aluminum foil, polyhydroxyethyl methacrylate, polydimethylsiloxane and silicon dioxide.

[0009] In one embodiment of the present invention, the hydrophilic polymer is dispersed in a medium to form a hydrophilic composition, and the hydrophilic composition is coated on the surface of the substrate by at least one method selected from spin coating, dip coating and spray coating.

[0010] In one embodiment of the present invention, the hydrophilic polymer content in the hydrophilic composition is 1 to 50% by weight.

[0011] In one embodiment of the present invention, the structure of the hydrophilic polymer is as shown in formula (I),

[0012]

[0013] Wherein, X is a unit derived from olefin, and its side chain has a hydrophilic group; and the ratio of a to b is 5:5 to 9:1.

[0014] In another embodiment of the present invention, the hydrophilic group is a hydroxyl group, a carboxylic acid group or a zwitterionic group.

[0015] In one embodiment of the present invention, the X is selected from at least one structure derived from the following monomers:

[0016]

[0017]

[0018] In another embodiment of the present invention, the hydrophilic polymer is of formula (I-1):

[0019]

[0020] The ratio of a to b is 5:5 to 7:3 and the weight average molecular weight of the hydrophilic polymer is in the range of 3000 to 25000 g / mol.

[0021] In one embodiment of the present invention, the temperature of the cross-linking reaction is 80 to 120° C., and the time of the cross-linking reaction is 0.5 to 15 hours.

[0022] The present invention further provides a substrate with a hydrophilic modified surface prepared by the method as described above, comprising: a substrate; and a hydrophilic modified layer chemically bonded to at least one surface of the substrate, wherein the hydrophilic modified layer comprises a hydrophilic polymer having units derived from N-hydroxymethyl acrylamide and units derived from olefins substituted with hydrophilic groups.

[0023] In one embodiment of the present invention, the material of the substrate is selected from the group consisting of copper foil, aluminum foil, polyhydroxyethyl methacrylate, polydimethylsiloxane and silicon dioxide.

[0024] In one embodiment of the present invention, the contact angle of the hydrophilic modified layer with water is 20 to 50 degrees.

[0025] In one embodiment of the present invention, the hydrophilic modified layer comprises a hydrophilic polymer having a unit derived from N-methylol acrylamide and a unit derived from an olefin substituted with a hydrophilic group, wherein the unit derived from the olefin substituted with a hydrophilic group is a structure derived from at least one of the following monomers:

[0026]

[0027] In another embodiment of the present invention, the hydrophilic polymer is of formula (I-1),

[0028]

[0029] The ratio of a to b is 5:5 to 7:3 and the weight average molecular weight of the hydrophilic polymer is in the range of 3000 to 25000 g / mol.

[0030] According to the present invention, a hydrophilic polymer containing units derived from N-hydroxymethyl acrylamide and units derived from olefins substituted with hydrophilic groups is cross-linked with the substrate to form a hydrophilic modified layer with chemical bonds, which can not only effectively improve the hydrophilicity of the surface, but also has better durability and water washability than existing modification technologies, and has application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Embodiments of the present invention are described by way of example with reference to the accompanying drawings:

[0032] Figure 1 is a schematic diagram of a substrate having a hydrophilic modified surface according to the present invention;

[0033] Figures 2A to 2B The Fourier transform infrared spectra of the hydrophilic modified layer of the substrate of Examples 1-1 to 1-2 of the present invention before and after the cross-linking reaction;

[0034] Figure 3 A comparison diagram of the vibration absorption peak areas of the hydroxyl groups at different crosslinking reaction times in the Fourier transform infrared spectroscopy analysis of the hydrophilic modified layer of the embodiment of the present invention; and

[0035] Figures 4A to 4H These are contact angle test graphs of water and the substrate surface before and after the hydrophilic treatment of the substrate surfaces of Examples 1-1 to 1-8 of the present invention, wherein the photo on the left side of each figure is the hydrophilic contact angle test before the hydrophilic treatment, and the photo on the right side is the hydrophilic contact angle test after the hydrophilic treatment.

[0036] Main component symbols

[0037] 1: Substrate with hydrophilic modified surface

[0038] 10: Base

[0039] 11: Hydrophilic modified layer. DETAILED DESCRIPTION

[0040] The following is an explanation of the embodiments of the present invention by specific specific examples, and those skilled in the art can easily understand the advantages and effects of the present invention from the contents described in this specification. The present invention can also be implemented or applied through other different embodiments, and the details in this specification can also be given different modifications and changes based on different viewpoints and applications without departing from the spirit described in the present invention. In addition, all ranges and values ​​herein are inclusive and combinable. Any numerical value or point falling within the range described herein, such as any integer, can be used as a minimum value or maximum value to derive a lower range, etc.

[0041] According to the present invention, a method for treating a substrate surface to be hydrophilic comprises: coating a hydrophilic polymer on a substrate surface having an active group; and causing the hydrophilic polymer to undergo a cross-linking reaction with the active group to obtain a substrate surface having hydrophilicity; wherein the hydrophilic polymer comprises a unit derived from N-hydroxymethyl acrylamide and a unit derived from an olefin substituted with a hydrophilic group.

[0042] Herein, the "active group" refers to any functional group or free radical that can undergo a cross-linking reaction with the unit derived from N-hydroxymethyl acrylamide of the hydrophilic polymer, and the source of the active group is not limited to the substrate itself, and includes those formed by activation treatment, especially surface activation treatment. In one embodiment, the active group may be a carboxylic acid group or a hydroxyl group; in one example, the active group is a hydroxyl group.

[0043] In one embodiment, the substrate having a reactive group used in the present invention may be poly(4-ethylphenol), poly(hydroxyethyl methacrylate), or a cross-linked copolymer having a hydroxyethyl methacrylate unit.

[0044] Herein, the "activation treatment" refers to a treatment technique that can generate the above-mentioned active groups on the substrate, such as plasma treatment, corona treatment, and light irradiation treatment. In one embodiment, the activation treatment is a plasma treatment, wherein the plasma gas is oxygen or air, and the operating conditions are preferably low pressure or normal pressure and room temperature to form the above-mentioned active groups.

[0045] In another embodiment, the substrate to be activated used in the present invention is a hydrophobic material, for example, one selected from the group consisting of silicon dioxide, polydimethylsiloxane (PDMS), polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polymethyl methacrylate (PMMA), polyurethane (PU), copper foil and aluminum foil.

[0046] In one embodiment, the substrate is copper foil, aluminum foil, silicon dioxide or polydimethylsiloxane; wherein the silicon dioxide can be selected from glass, quartz sheet or a silicon dioxide layer formed on a wafer.

[0047] By selecting and activating the active groups on the surface of the substrate, the bonding strength between the substrate and the hydrophilic polymer interface is improved, and the quality of the hydrophilic modified layer covering the surface of the substrate is further optimized, thereby exhibiting excellent wear resistance.

[0048] Regarding the method of coating the hydrophilic polymer on the surface of the substrate, any appropriate known coating technology can be used, such as: roller coating, spin coating, wire rod coating, dip coating, curtain coating, spray coating, doctor blade coating, slit coating, but not limited thereto.

[0049] In order to uniformly shape the hydrophilic polymer coated on the surface of the substrate, the hydrophilic polymer is uniformly and stably dispersed in the medium to form a hydrophilic composition. In one embodiment, the hydrophilic composition can directly use a hydrophilic polymer solution product obtained by polymerizing N-methylol acrylamide monomer and a hydrophilic monomer; or a dispersion of hydrophilic polymer pellets containing units derived from N-methylol acrylamide and units derived from olefins substituted with hydrophilic groups dissolved in a solvent. In one embodiment, the solvent for dissolving the hydrophilic polymer is preferably methanol, ethanol or an aqueous medium; wherein the aqueous medium is generally water, usually deionized water.

[0050] In the present invention, a hydrophilic polymer is dispersed in an aqueous medium to form a hydrophilic composition, and is coated on the surface of the substrate by at least one method selected from spin coating, dip coating and spray coating; in particular, when the coating is performed by spin coating, the spin coating speed is set in the range of 500 to 3000 rpm so that the hydrophilic composition forms a layer of uniform thickness on the surface of the substrate.

[0051] In one embodiment, the hydrophilic polymer content of the hydrophilic composition is 1 to 50 wt %; in other embodiments, the hydrophilic polymer content of the hydrophilic composition can be 3, 5, 7, 10, 15, 20, 25, 30, 35, 40 or 45 wt %, and is not limited thereto.

[0052] In another embodiment, when the hydrophilic composition uses water as the medium, the content of the hydrophilic polymer in the hydrophilic composition is 1 to 50 wt %.

[0053] In another embodiment, the hydrophilic composition may optionally contain other auxiliary agents, such as reaction aids, cosolvents, thickeners, UV absorbers, antimicrobial agents, etc., depending on the subsequent application and functional requirements of the substrate.

[0054] Herein, the "crosslinking reaction" refers to a chemical reaction induced by heat, acid, alkali or radiation treatment, which forms chemical bonds between the hydrophilic polymers in the hydrophilic modified layer and between the hydrophilic modified layer and the substrate interface. In the present invention, the crosslinking reaction procedure can be carried out simultaneously with the coating process, or after the coating process is completed.

[0055] In one embodiment of the present invention, the cross-linking reaction is a thermal cross-linking reaction, and the operating environment of the thermal cross-linking reaction is carried out under conditions below normal pressure, and particularly preferably under a vacuum state to accelerate the efficiency of the reaction; in one embodiment, the absolute pressure of the thermal cross-linking reaction is in the range of less than 0.1 MPa; in another embodiment, the pressure of the thermal cross-linking reaction is lower than 0.5 Pa.

[0056] In another embodiment, the operating temperature of the cross-linking reaction is higher than 80° C., that is, there is a basic degree of reaction effect, and the preferred cross-linking temperature range is 80 to 120° C. In one embodiment, when the cross-linking temperature is in the range of 80 to 120° C., the cross-linking reaction time is 0.5 to 15 hours, that is, chemical bonds are formed.

[0057] In other embodiments, the crosslinking reaction temperature can be 85, 90, 95, 100, 105, 110 or 115° C.; the crosslinking reaction time can be 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 7, 10 or 12 hours, and are not limited thereto.

[0058] In one embodiment, when the coating is performed by dip coating, the cross-linking reaction can be a two-step procedure, including: a first cross-linking reaction carried out simultaneously with the dip coating process, and a second cross-linking reaction carried out successively after the dip coating process, wherein the temperature of the first cross-linking reaction is 90 to 120°C, and the reaction time is 0.5 to 3 hours; the temperature of the second cross-linking reaction is 80 to 120°C, and the reaction time is 1 to 12 hours.

[0059] In another embodiment, the cross-linking reaction is performed after the spin coating process is completed, and the cross-linking reaction temperature is 80 to 120° C., and the reaction time is 1 to 12 hours.

[0060] According to the cross-linking reaction of the present invention, a chemical bond can be formed between the substrate and the interface of the hydrophilic modification layer, thereby making the substrate prepared by the present invention have a more durable hydrophilic modification surface than the existing modification technology.

[0061] In the present invention, the hydrophilic polymer is composed of at least two or more repeating structural units, and can be optionally arranged in random, alternating, block, etc. In one embodiment, the hydrophilic polymer is a random copolymer composed of units derived from N-hydroxymethyl acrylamide and units derived from olefins substituted with hydrophilic groups.

[0062] In one embodiment, the hydrophilic group comprises a hydroxyl group, a carboxylic acid group, or a zwitterionic group.

[0063] In one embodiment, the hydrophilic polymer has a structure as a random copolymer as shown in formula (I),

[0064]

[0065] Wherein, X is a unit derived from olefin, and its side chain has a hydrophilic group, and the ratio of a to b is 5:5 to 9:1.

[0066] In other embodiments, the ratio of a to b in the hydrophilic polymer may be 5:5, 6:4, 7:3 or 8:2, but is not limited thereto.

[0067] In another embodiment, the hydrophilic polymer further includes at least one additional unit in addition to the unit derived from N-methylolacrylamide and the unit derived from an olefin substituted with a hydrophilic group; that is, the hydrophilic polymer may further include two, three, four or more additional units different from the unit derived from N-methylolacrylamide and the unit derived from an olefin substituted with a hydrophilic group.

[0068] The above-mentioned unit derived from the olefin substituted with a hydrophilic group is selected from at least one structure derived from the following monomers, and a suitable unit is selected according to the actual application:

[0069]

[0070]

[0071] For example, if the prepared substrate with a hydrophilic modified surface is to be applied to contact lenses for eyes, the unit derived from the olefin substituted with a hydrophilic group can be derived from the A-5 monomer structure, which not only provides good wettability, but also provides the effect of increasing the wearing comfort and stability of the user; if the prepared substrate with a hydrophilic modified surface is applied to lithium-ion battery electrodes, it also has the effect of increasing the stability of performance.

[0072] In another embodiment, the structure of the hydrophilic polymer of the present invention is a random copolymer as shown in formula (I-1);

[0073]

[0074] The ratio of a to b is 5:5 to 7:3 and the weight average molecular weight is in the range of 3000 to 25000 g / mol.

[0075] In other embodiments, the weight average molecular weight of the hydrophilic polymer of formula (I-1) can be 5000, 7000, 10000, 12000, 14000, 16000, 18000, 20000, 22000 or 24000 g / mol, but is not limited thereto.

[0076] The substrate with a hydrophilic modified surface is obtained by the preparation method of the present invention, comprising: a substrate; and a hydrophilic modified layer chemically bonded to at least one surface of the substrate.

[0077] The hydrophilicity is determined by measuring the contact angle of a water droplet. In the present invention, the contact angle measurement results of the layer body in a dry state are observed; in one embodiment, the contact angle of the hydrophilic modified layer with water is 20 to 50 degrees.

[0078] In other embodiments, the contact angle of the hydrophilic modified layer with water can be 22, 25, 27, 30, 32, 35, 37, 40, 42, 45 or 47 degrees, but is not limited thereto.

[0079] See also Figure 1 , illustrating the substrate 1 with a hydrophilic modified surface of the present invention, comprising: a substrate 10; and a hydrophilic modified layer 11 on the surface of the substrate, wherein the substrate is selected from the group consisting of copper foil, aluminum foil, polyhydroxyethyl methacrylate, polydimethylsiloxane and silicon dioxide; the hydrophilic modified layer comprises a hydrophilic polymer having units derived from N-hydroxymethyl acrylamide and units derived from olefins substituted with hydrophilic groups.

[0080] In another embodiment, the unit derived from an olefin substituted with a hydrophilic group is a structure derived from at least one of the following monomers:

[0081] and

[0082] In another embodiment of the present invention, the hydrophilic polymer is a random copolymer of formula (I-1):

[0083]

[0084] The ratio of a to b is 5:5 to 7:3 and the weight average molecular weight is in the range of 3000 to 25000 g / mol.

[0085] See also Figures 2A to 2B, is a Fourier transform infrared spectrum of the hydrophilic modified layer of the substrate prepared in the present invention before and after the cross-linking reaction, and the dotted line frame in the figure (wave number is 3300 to 3700 cm -1 The range) is the vibration absorption of the hydroxyl group of the unit derived from N-methylol acrylamide of the hydrophilic polymer in the hydrophilic modified layer; and Figure 3 In the experiment, the areas of the vibration absorption peaks of the hydroxyl groups at different crosslinking reaction times are compared. The results show that after the crosslinking reaction, the absorption of the hydroxyl groups of the hydrophilic polymer in the hydrophilic modified layer is significantly reduced, and as the crosslinking reaction time increases, the vibration absorption of the hydroxyl groups of the hydrophilic polymer also decreases. This proves that the crosslinking reaction forms new chemical bonds between the hydrophilic polymers and between the hydrophilic polymer and the substrate in the hydrophilic modified layer, and as the degree of the crosslinking reaction increases, more chemical bonds are formed, so that a more lasting hydrophilic property can be exhibited.

[0086] The features and effects of the present invention are further described in detail below through specific examples, but the scope of the present invention is not limited by the examples.

[0087] Synthesis Example: Synthesis of Hydrophilic Polymer (I-1)

[0088] First, N-hydroxymethyl acrylamide monomer (0.0105 mol) and initiator azobisisobutyronitrile (AIBN, 0.00014 mol) were placed in a double-necked round-bottom flask and connected to a vacuum system for drying. Furthermore, a methanol / water mixed solvent with a volume ratio of 7:1 was prepared, and 3-[[2-(acryloyloxy)ethyl]dimethylammonio]propane-1-sulfonate monomer (0.0245 mol) was dissolved in the mixed solvent in a single-necked round-bottom flask, and the reaction solution in the single-necked round-bottom flask was purged with argon for 30 minutes to remove dissolved oxygen in the reaction solution.

[0089] Next, the reaction solution in the single-neck round-bottom flask was transferred to the double-neck round-bottom flask to mix all the raw materials. After they were completely dissolved, the double-neck round-bottom flask was transferred to a 65° C. oil bath for polymerization. Finally, the mixture in the double-neck round-bottom flask was cooled and exposed to air to stop the polymerization reaction. The reaction time was 24 hours. Subsequently, a dialysis membrane with a molecular weight cutoff of 10,000 was used to separate and remove impurities in the mixture, thereby obtaining a random copolymer as shown in the following formula (I-1), and the prepared hydrophilic polymer was stored in deionized water.

[0090]

[0091] Then, the weight average molecular weight and polydispersity index (PDI value) of the above products were measured. For the analysis of molecular weight and polydispersity index, gel permeation chromatography (GPC, Waters, 1515) was used for detection, and the operating conditions were set as follows: (1) mobile phase: 1 ml / min, THF; (2) detector model: Waters 2414 refractive index detector; detection temperature: 40°C; (3) concentration of the product used for GPC detection: 1.5 mg / ml; (4) injection volume: 200 μL; (5) chromatographic column model: Watercolumn 7.8x300 mm.

[0092] According to the above analysis, the product has a weight average molecular weight of 23,598, a number average molecular weight of 13,110, and a PDI value of 1.8.

[0093] Example 1-1: Preparation of a substrate having a hydrophilically modified surface

[0094] First, a polydimethylsiloxane (PDMS) substrate is placed in a plasma chamber, and its surface is activated by plasma generated by dry air at room temperature and pressure. The set power of the plasma is 120W, and the operation time is 30 seconds.

[0095] Secondly, the hydrophilic polymer prepared in Synthesis Example 1 was prepared into a hydrophilic composition containing 1 wt % of the hydrophilic polymer using water as a solvent; the prepared hydrophilic composition was formed into a hydrophilic modified layer of uniform thickness on the surface of the activated PDMS substrate by a spin coating device at a rotation speed of 1000 rpm.

[0096] Next, the coated substrate was placed in an oven and heated to 90° C. The absolute pressure was set under vacuum conditions to perform a cross-linking reaction for 12 hours, thereby obtaining a hydrophilically modified substrate surface.

[0097] Finally, the substrate prepared above was subjected to the following tests and analyses:

[0098] (1) Qualitative analysis of surface bonding: After surface modification, the infrared spectrum of the surface was measured using an attenuated total reflection Fourier transform infrared spectrometer (ATR-FTIR, PerkinElmer; Spectrum Two). The substrate without solution coating was used as the baseline to observe the changes in the hydroxyl groups (wave number 3300 to 3700 cm -1 range), and record the results in Figure 2A .

[0099] (2) Surface hydrophilicity test: After the surface modification is completed, the surface is first cleaned by rinsing with water for 1 to 12 hours and then dried under a pressure of less than 0.1 MPa and room temperature. Then, the contact angle in the dry state is measured using a contact angle meter (Kyowa Interface Science Co., Ltd.; MCA-3) and the results are recorded in Table 1 and Figure 4A .

[0100] (3) Durability test:

[0101] (3-1) Long-term hydrophilicity test: The prepared substrate was stored in an environment with a temperature of 25 to 30° C. and a humidity of 60 to 90%. After 6 months, the contact angle of the substrate surface was measured according to the above-mentioned surface hydrophilicity test method, and the results are recorded in Table 2.

[0102] (3-2) Immersion test: After the prepared substrate is placed in an environment with a temperature of 25 to 30°C and a humidity of 60 to 90% for 6 months, the substrate is immersed in deionized water for 1 hour and dried at room temperature and a pressure less than 0.1 MPa. The contact angle is then measured according to the contact angle measurement method of (2) above, and the results are recorded in Table 2.

[0103] (3-3) Water washing test: After the prepared substrate is placed in an environment with a temperature of 25 to 30°C and a humidity of 60 to 90% for 6 months, the substrate is placed in a container containing deionized water and cleaned by hand-shaking for 5 to 10 minutes; then, the substrate is dried at room temperature and a pressure of less than 0.1 MPa, and then the contact angle measurement method (2) is used to measure the contact angle, and the results are recorded in Table 2.

[0104] Example 1-2: Effect of substrate material changes

[0105] The substrate preparation method is the same as that of Example 1-1, but the polydimethylsiloxane substrate is replaced by the silicon dioxide layer of the wafer; then, the prepared substrate is subjected to surface bonding, hydrophilicity analysis and durability test, and the results are recorded in Figure 2B , Figure 4B , Table 1 and Table 2.

[0106] Examples 1-3 to 1-7: Effect of substrate material changes

[0107] The substrate preparation method is the same as that of Example 1-1, but the substrate materials are replaced with copper foil, aluminum foil, glass, quartz and polyethylene terephthalate respectively; then, the prepared substrates are subjected to surface bonding and hydrophilicity analysis, and the results are recorded in Figures 4C to 4G , Table 1 and Table 2.

[0108] Example 1-8: Effect of substrate material changes

[0109] The substrate preparation method is the same as that of Example 1-1, except that the polydimethylsiloxane substrate is replaced by a poly(hydroxyethyl methacrylate) substrate having a cross-linked structure, and the spin coating process is directly performed without surface activation treatment; then, the prepared substrate is subjected to surface bonding, hydrophilicity analysis and durability test, and the results are recorded in Figure 4H , Table 1 and Table 2.

[0110] Example 2-1: Effect of different coating methods

[0111] The hydrophilic polymer prepared in Synthesis Example 1 was prepared into a hydrophilic composition containing 1 wt% of the hydrophilic polymer using water as a solvent; a cross-linked poly(hydroxyethyl methacrylate) substrate was immersed in the hydrophilic composition for 3 hours at a temperature of 90°C, so that the hydrophilic composition was deposited on the surface of the substrate to form a hydrophilic modified layer.

[0112] Next, the coated substrate was placed in an oven and the temperature was set to 90° C., and a cross-linking reaction was performed for 12 hours under vacuum conditions to obtain a hydrophilically modified substrate surface. The substrate obtained above was analyzed according to the test method of Example 1-1 and recorded in Table 1.

[0113] Comparative Examples 1 to 8: Plasma Treatment

[0114] The various substrates listed in Table 1 were placed in a plasma chamber, and their surfaces were activated by plasma generated by dry air at room temperature and pressure. The plasma power was set to 120 W and the operation time was 30 seconds, thereby obtaining a hydrophilically modified substrate surface.

[0115] Next, the substrate prepared above was analyzed according to the testing method of Example 1-1 and recorded in Table 1 and Table 2.

[0116] Table 1

[0117]

[0118]

[0119] Table 2

[0120]

[0121] In summary, the method for treating the surface of a substrate with hydrophilicity of the present invention uses a hydrophilic polymer containing units derived from N-hydroxymethyl acrylamide and units derived from an olefin substituted with a hydrophilic group to undergo a cross-linking reaction with the substrate to form a substrate having a chemically bonded hydrophilic modified layer. This method can not only effectively improve the hydrophilicity of the surface, but also has better durability and water washability than existing modification technologies, and has application prospects.

[0122] The above embodiments are only illustrative and are not intended to limit the present invention. Any person skilled in the art may modify and change the above embodiments without violating the spirit and scope of the present invention. Therefore, the scope of protection of the present invention is defined by the claims attached to the present invention, and as long as it does not affect the effect and implementation purpose of the present invention, it should be included in the disclosed technical content.

Claims

1. A method for hydrophilic treatment of a substrate surface, comprising: The hydrophilic polymer is coated on the surface of the substrate having the active groups; as well as Allowing the hydrophilic polymer to undergo a cross-linking reaction with the active group to obtain a hydrophilic substrate surface; The hydrophilic polymer comprises a unit derived from N-hydroxymethyl acrylamide and a unit derived from an olefin substituted with a hydrophilic group. Wherein, the structure of the hydrophilic polymer is as shown in formula (I), Wherein, the X is selected from at least one structure derived from the following monomers; and The ratio of a to b is 5:5 to 9:1; and 2. The method of claim 1, wherein: The substrate surface with active groups is formed by activation treatment.

3. The method of claim 2, wherein: The activation process is a plasma process, and the plasma gas is oxygen or air.

4. The method of claim 1, wherein: The active group is a hydroxyl group.

5. The method for treating a substrate surface as claimed in claim 1, wherein: The material of the substrate is selected from the group consisting of copper foil, aluminum foil, polyhydroxyethyl methacrylate, polydimethylsiloxane and silicon dioxide.

6. The method of claim 1, wherein: The hydrophilic polymer is dispersed in a medium to form a hydrophilic composition, and the hydrophilic composition is coated on the surface of the substrate by at least one method selected from spin coating, dip coating and spray coating.

7. The method of claim 6, wherein: The content of the hydrophilic polymer in the hydrophilic composition is 1 to 50% by weight.

8. The method of claim 1, wherein: The hydrophilic polymer is of formula (I-1): The ratio of a to b is 5:5 to 7:3, and the weight average molecular weight of the hydrophilic polymer is in the range of 3000 to 25000 g / mol.

9. The method of claim 1, wherein: The temperature of the cross-linking reaction is 80 to 120° C., and the time of the cross-linking reaction is 0.5 to 15 hours.

10. A substrate having a hydrophilic modified surface prepared by the method according to claim 1, comprising: substrate; as well as a hydrophilic modification layer chemically bonded to at least one surface of the substrate, wherein the hydrophilic modification layer comprises a hydrophilic polymer having units derived from N-hydroxymethyl acrylamide and units derived from an olefin substituted with a hydrophilic group; Wherein, the unit derived from the olefin substituted with a hydrophilic group is derived from at least one structure of the following monomers: and 11. The substrate of claim 10, wherein The material of the substrate is selected from the group consisting of copper foil, aluminum foil, polyhydroxyethyl methacrylate, polydimethylsiloxane and silicon dioxide.

12. The substrate of claim 10, wherein The contact angle of the hydrophilic modified layer with water is 20 to 50 degrees.

13. The substrate of claim 10, wherein The hydrophilic polymer has a structure of formula (I-1), The ratio of a to b is 5:5 to 7:3, and the weight average molecular weight of the hydrophilic polymer is in the range of 3000 to 25000 g / mol.

Citation Information

Patent Citations

  • A plasma-photochemical method for grafting carboxyl groups onto cell culture surfaces

    CN102276866A

  • Contact lenses comprising water soluble N-(2 hydroxyalkyl) (meth)acrylamide polymers or copolymers

    CN104321356A

  • Hydrophilic modification method of polyethylene material, hydrophilic polyethylene material and reaction liquid for hydrophilic modification of polyethylene material

    CN113429621A

  • Polyelectrolyte hydrogel coating with super-strong substrate adhesion performance and preparation method of polyelectrolyte hydrogel coating

    CN113842507A

  • Surface treatment of medical devices iwth reactive hydrophilic polymers

    CN1376270A