A method for preparing high-performance neodymium iron boron magnets
By employing a eutectic ratio of rare earth elements and metal particles in the preparation of NdFeB magnets and forming amorphous alloy strips through multiple melting processes, combined with the deposition and heat treatment of amorphous diffusion sources, the problems of complex NdFeB magnet preparation processes and unstable diffusion efficiency have been solved, thus achieving efficient and stable production of high-performance NdFeB magnets.
Patent Information
- Application Number
- CN202310594680.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-05-24
AI Technical Summary
Existing neodymium iron boron magnets have complex manufacturing processes and unstable diffusion efficiency, resulting in insufficient magnetic properties and serious waste of heavy rare earth elements.
By forming amorphous alloy strips through multiple melting and high-speed cooling after the eutectic composition of rare earth elements and metal particles is determined, combined with the deposition and heat treatment of amorphous diffusion sources, the uniform distribution and diffusion of rare earth elements on the magnet surface are promoted, the diffusion time is shortened and the amount of rare earth elements used is saved.
It significantly improves grain boundary diffusion efficiency, shortens the process flow, and produces high-performance NdFeB magnets that are easy to mass-produce and have stable performance.
Smart Images

Figure CN116666097B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of neodymium iron boron permanent magnet material preparation, and more specifically, to a method for preparing high-performance neodymium iron boron magnets. Background Technology
[0002] With the development trend of energy conservation and emission reduction in fields such as new energy vehicles, wind power generation, and home appliances, sintered NdFeB permanent magnets, as a core material in these fields, are of paramount importance in achieving high efficiency and energy saving.
[0003] Grain boundary diffusion technology, as a method to significantly enhance the magnetic properties of magnets using small amounts of heavy rare earth elements, has attracted widespread attention from industry and academia. Currently, the diffusion sources used in grain boundary diffusion technology are mainly fluorides, hydrides, or heavy rare earth alloys. However, the mass production of fluorides faces limitations, and the hydrogen gas used in the preparation of hydrides poses certain risks. The preparation technologies for the currently favored heavy rare earth alloys are inconsistent, and their diffusion efficiency is unstable, thus limiting their mass production and affecting their applications. Existing alloy diffusion sources, by preparing strips through the proportional melting of heavy rare earth and non-rare earth elements for grain boundary diffusion, neglect the influence of the alloy strip state on grain boundary diffusion, resulting in prolonged diffusion time and waste of heavy rare earth elements. Summary of the Invention
[0004] Therefore, in order to solve the problems of complex fabrication process, unstable diffusion efficiency, and insufficient magnetic properties of NdFeB magnets in the prior art, this invention provides a method for preparing high-performance NdFeB magnets, the specific technical solution of which is as follows: A method for preparing a high-performance neodymium iron boron magnet includes the following steps: Based on the binary or ternary alloy phase diagram of rare earth elements and metals, the eutectic composition of rare earth elements and metals is found. Rare earth element blocks and metal particles are mixed in proportion, and then the rare earth element blocks and metal particles are stacked. The first vacuum is drawn, and the melting process is carried out under the protection of argon atmosphere. After solidification, it is flipped to the other side and melted again. This process is repeated several times. After cooling, the alloy ingot is obtained. The alloy ingot is polished and sheared, then placed in a quartz tube for a second vacuum treatment. Argon gas is then introduced for protection, so that the pressure difference between the furnace body and the outside of the furnace is 0.05 MPa to 0.20 MPa. The rotation speed of the copper roller is adjusted to 25 m / s to 60 m / s. Then, the induction coil heating function is turned on to heat the alloy ingot until it is completely melted. Immediately after that, it is spray-cast to obtain an amorphous alloy strip. The amorphous alloy strip is mechanically crushed and then ground to obtain coarse powder. After the coarse powder is subjected to a first ball milling process, a second ball milling process, and a third ball milling process, it is then dried and sieved to obtain amorphous powder. The amorphous powder, alcohol, and PVB adhesive are mixed evenly to obtain a suspension; The suspension is ultrasonically vibrated and then deposited on the surface of a magnet. After vacuum drying, the deposited amorphous diffusion source magnet is placed in a hot press furnace with a vacuum of 3×10⁻² Pa to 8×10⁻⁵ Pa and a holding temperature of 400 to 500 °C. During this period, a pressure of 0.5 to 10 MPa is applied to allow the amorphous diffusion source to relax under the combined effects of amorphous transformation temperature and pressure, promoting the uniform distribution of the diffusion source on the magnet surface. Then, diffusion is carried out at 900 °C to 950 °C for 9 to 11 hours, followed by tempering at 450 °C to 550 °C for 3 to 4 hours to obtain a high-performance NdFeB magnet.
[0005] Furthermore, the rare earth element block is one or a mixture of two or more of Dy, Tb, Pr, Nd, Ho, La, Ce, Y, and Sm.
[0006] Furthermore, the metal particles are one or a mixture of two or more of Al, Cu, Ga, Mg, Zn, Sn, Mn, Co, and Ni.
[0007] Furthermore, the mass ratio of the rare earth element block to the metal particles is (1.5~9):1. Furthermore, the vacuum level of the first evacuation is 3 × 10⁻⁶. -2 Pa ~ 8×10 -5 Pa.
[0008] Furthermore, the size of the shearing process is 20 × 10 mm. 2 .
[0009] Furthermore, the vacuum degree of the second vacuum evacuation is 3×10⁻⁶. -2 Pa ~ 8×10 -5 Pa.
[0010] Further, in the first ball milling process, each grinding ball weighs 8g to 20g, and is mixed and milled in a ball-to-material ratio of 6:1 to 2:1 in a ball mill jar. Alcohol is added until it completely submerges the grinding balls and coarse powder. The ball mill speed is then adjusted to 200 r / min to 350 r / min, and the milling time is 20 min to 40 min. The alcohol in the ball mill jar is then poured out, and the fine powder floating in the alcohol is sieved out. The second ball milling process involves continuing to add alcohol until it completely submerges the grinding balls and coarse powder, adjusting the ball mill speed to 200 r / min to 350 r / min, and milling for 20 min to 40 min. After min, pour out the alcohol from the ball mill jar and sift out the fine powder floating in the alcohol; the third ball milling process is as follows: use ball milling beads with a single mass of 0.5g to 2g, add them to the ball mill jar according to the ball-to-material mass ratio of 6:1 to 2:1 for mixing and ball milling, continue to add alcohol to cover the ball milling beads and coarse powder, then adjust the ball mill speed to 200 r / min to 350 r / min, and the ball milling time is 10 min to 30 min, and then remove the ball milling beads.
[0011] Furthermore, the mass ratio of the amorphous powder, alcohol, and PVB adhesive is 1:1:0.03.
[0012] Furthermore, the vacuum drying temperature is 10℃~40℃, and the time is 20min~60min.
[0013] The aforementioned method significantly shortens diffusion time and saves rare earth element usage by depositing an amorphous diffusion source on the magnet surface, resulting in high-performance NdFeB magnets with low rare earth element usage. The preparation method presented in this application is efficient, has a short process, and is easy to mass-produce. It involves melting rare earth elements with metals to form an alloy, followed by high-speed cooling to form amorphous flakes or powders. Utilizing the metastable state, relaxation characteristics, and high fluidity of the amorphous alloy, element migration during heat treatment is promoted, thereby significantly improving grain boundary diffusion efficiency and shortening the process flow. The sintered NdFeB magnets prepared after diffusion through the amorphous diffusion source exhibit stable performance and are easy to promote and apply. Attached Figure Description
[0014] Figure 1 These are the XRD diffraction patterns of low-melting alloy powder at different spinning speeds in Example 1 of this invention; Figure 2 This is a schematic diagram of the production process using the spraying method in Embodiment 1 of the present invention. Detailed Implementation
[0015] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to its embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and do not limit the scope of protection of the invention.
[0016] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0017] A method for preparing a high-performance neodymium iron boron magnet according to one embodiment of the present invention includes the following steps: Based on the binary or ternary alloy phase diagram of rare earth elements and metals, the eutectic composition of rare earth elements and metals is found. Rare earth element blocks and metal particles are mixed in proportion, and then the rare earth element blocks and metal particles are stacked. The first vacuum is drawn, and the melting process is carried out under the protection of argon atmosphere. After solidification, it is flipped to the other side and melted again. This process is repeated several times. After cooling, the alloy ingot is obtained. The alloy ingot is polished and sheared, then placed in a quartz tube for a second vacuum treatment. Argon gas is then introduced for protection, so that the pressure difference between the furnace body and the outside of the furnace is 0.05 MPa to 0.20 MPa. The rotation speed of the copper roller is adjusted to 25 m / s to 60 m / s. Then, the induction coil heating function is turned on to heat the alloy ingot until it is completely melted. Immediately after that, it is spray-cast to obtain an amorphous alloy strip. The amorphous alloy strip is mechanically crushed and then ground to obtain coarse powder. After the coarse powder is subjected to a first ball milling process, a second ball milling process, and a third ball milling process, it is then dried and sieved to obtain amorphous powder. The amorphous powder, alcohol, and PVB adhesive are mixed evenly to obtain a suspension; The suspension was ultrasonically vibrated and then deposited onto the surface of a magnet. After vacuum drying, the deposited amorphous diffusion source magnet was placed in a hot press furnace with a vacuum of 3×10⁻² Pa to 8×10⁻⁵ Pa and a holding temperature of 400 to 500 °C. During this period, a pressure of 0.5 to 10 MPa was applied to allow the amorphous diffusion source to relax under the combined effects of amorphous transformation temperature and pressure, promoting the uniform distribution of the diffusion source on the magnet surface. Diffusion was carried out at 900 °C to 950 °C for 9 to 11 hours, followed by tempering at 450 °C to 550 °C for 3 to 4 hours to obtain a high-performance NdFeB magnet.
[0018] In one embodiment, the rare earth element block is one or a mixture of two or more of Dy, Tb, Pr, Nd, Ho, La, Ce, Y, and Sm.
[0019] In one embodiment, the metal particles are one or a mixture of two or more of Al, Cu, Ga, Mg, Zn, Sn, Mn, Co, and Ni.
[0020] In one embodiment, the purity of the rare earth element block is greater than or equal to 99.9%.
[0021] In one embodiment, the purity of the metal particles is greater than or equal to 99.99%.
[0022] In one embodiment, the mass ratio of the rare earth element block to the metal particles is 1.5 to 9:1. In one embodiment, the vacuum level of the first evacuation is 3 × 10⁻⁶. -2 Pa ~ 8×10 -5 Pa.
[0023] In one embodiment, the cutting process has a size of 20 × 10 mm. 2 .
[0024] In one embodiment, the mechanical crushing process yields 1mm fragments.
[0025] In one embodiment, the vacuum level of the second evacuation is 3 × 10⁻⁶. -2 Pa ~ 8×10 -5 Pa.
[0026] In one embodiment, the first ball milling process involves adding individual grinding balls weighing 8g to 20g to a grinding jar at a ball-to-material ratio of 6:1 to 2:1 for mixing and grinding. Alcohol is added until it completely submerges the grinding balls and coarse powder. The ball mill speed is then adjusted to 200 r / min to 350 r / min, and the milling time is 20 min to 40 min. The alcohol is then poured out of the grinding jar, and the fine powder floating in the alcohol is sieved out. The second ball milling process involves continuing to add alcohol until it completely submerges the grinding balls and coarse powder, adjusting the ball mill speed to 200 r / min to 350 r / min, and milling for 20 min to 40 min. After min, pour out the alcohol from the ball mill jar and sift out the fine powder floating in the alcohol; the third ball milling process is as follows: use ball milling beads with a single mass of 0.5g~2g, mix them with the material in a ball-to-material mass ratio of 6:1~2:1 and add them to the ball mill jar for mixing and ball milling, continue to add alcohol to cover the ball milling beads and coarse powder, then adjust the ball mill speed to 200 r / min~350 r / min, and the ball milling time is 10min~30min, and then remove the ball milling beads.
[0027] In one embodiment, the mass ratio of the amorphous powder, alcohol, and PVB adhesive is 1:1:0.03. In one embodiment, the vacuum drying temperature is 10°C to 40°C and the time is 20 min to 60 min.
[0028] In one embodiment, the thickness of the amorphous alloy strip is 5 μm to 200 μm.
[0029] In one embodiment, the sieving process yields amorphous powder with a particle size of less than or equal to 100 μm.
[0030] In one embodiment, the particle size of the amorphous powder is 20 μm to 50 μm.
[0031] The aforementioned method significantly shortens diffusion time and saves rare earth element usage by depositing an amorphous diffusion source on the magnet surface, resulting in high-performance NdFeB magnets with low rare earth element usage. The preparation method presented in this application is efficient, has a short process, and is easy to mass-produce. It involves melting rare earth elements with metals to form an alloy, followed by high-speed cooling to form amorphous flakes or powders. Utilizing the metastable state, relaxation characteristics, and high fluidity of the amorphous alloy, element migration during heat treatment is promoted, thereby significantly improving grain boundary diffusion efficiency and shortening the process flow. The sintered NdFeB magnets prepared after diffusion through the amorphous diffusion source exhibit stable performance and are easy to promote and apply.
[0032] The implementation schemes of the present invention will now be described in detail with reference to specific embodiments.
[0033] Example 1: A method for preparing a high-performance neodymium iron boron magnet includes the following steps: Step 1: Based on the Nd-Cu binary alloy phase diagram, determine the binary eutectic composition of Nd-Cu as Nd. 84 Cu 16 (by mass) Rare earth element Nd with a purity of 99.9% is added during the preparation process, along with elemental Cu particles with a purity of 99.99%. The surface of the rare earth Nd block is ground and polished to remove the oxide scale before weighing. Step 2: Melting is carried out using a high-vacuum electric arc melting furnace. The raw materials are arranged with rare earth Nd blocks at the bottom and elemental Cu particles at the top. After arrangement, a vacuum is drawn to a degree higher than 8×10⁻⁶. -3 Pa, and then under the protection of argon atmosphere, the alloy raw material is heated and melted to a molten state. After it solidifies, it is flipped to the other side and melted again to obtain an alloy ingot. After it cools, the melting is repeated 4 times to ensure its composition is uniform. After the alloy ingot cools, it is taken out for use. Step 3: Use a sander to clean the oxide scale off the surface of the alloy ingot, and then use a shearing machine to cut it into pieces of 20×10 mm size. 2 Small pieces of varying sizes are placed side-by-side in a quartz tube, which is then installed in a high-vacuum belt spinning device. After sealing the furnace body, preparations are made to evacuate the vacuum, raising the vacuum level to above 8 × 10⁻⁶. -3 Pa, after the vacuum degree reaches the required level, shut down the vacuum system to prepare for gas distribution in the furnace body, introduce argon gas into the furnace body for protection, make the pressure difference between the furnace body and the outside pressure 0.05 MPa, adjust the copper roller speed to 40 m / s, and then turn on the induction coil heating function to heat the alloy ingot to complete melting and immediately perform spray casting to obtain amorphous alloy strips. Step 4: Mechanically crush the amorphous alloy strip into 1 mm fragments, then grind the fragments, and after sieving, select coarse powder with a particle size of 800 μm for later use. Step 5: The coarse powder is ball-milled using a planetary ball mill. The ball milling process is carried out in three steps: The first ball milling process involves adding 8g of individual grinding beads to a grinding jar at a ball-to-material ratio of 4:1 for mixing and grinding. Alcohol is added until it completely covers the grinding beads and coarse powder. The ball mill speed is then adjusted to 300 r / min, and the grinding time is 30 minutes. The alcohol is then poured out of the grinding jar, and the fine powder floating in the alcohol is sieved out. The second ball milling process involves adding alcohol again to cover the grinding beads and coarse powder, adjusting the ball mill speed to 300 r / min, and grinding for 30 minutes. The alcohol is then poured out of the grinding jar, and the fine powder floating in the alcohol is sieved out. The third ball milling process involves using 0.5g grinding beads, mixed at a ball-to-material ratio of 4:1, and added to a grinding jar for mixing and grinding. Alcohol is then added again to cover the grinding beads and coarse powder, and the ball mill speed is adjusted to 300 r / min, and the grinding time is 20 minutes. The grinding beads are then removed.
[0034] Step 6: After removing the ball mill jar, place it in a vacuum drying oven for drying at a temperature of 30°C for 40 minutes. After drying, remove the powder and sieve it to obtain amorphous powder with a particle size of 25 μm for later use. Step 7: Mix amorphous powder, alcohol and PVB adhesive in a mass ratio of 1:1:0.03 evenly to prepare a suspension. After ultrasonic vibration for 5 minutes, deposit it on the magnet surface by spraying or impregnation. After vacuum drying, it is ready for use. Then, according to the grain boundary diffusion process, diffuse at 900℃ for 10 hours and temper at 500℃ for 3 hours to obtain a high-performance magnet.
[0035] Example 2: The difference between Example 2 and Example 1 is that the grain boundary diffusion process in Example 2 is: diffusion at 920°C for 9 hours, followed by tempering at 520°C for 4 hours, and the rest is the same as in Example 1.
[0036] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not use the binary eutectic composition of NdCu in step 1 as the nominal composition, but instead uses a composition that deviates from its eutectic composition. The other processes are the same as in Example 1.
[0037] Comparative Example 2: The difference between Comparative Example 2 and Example 1 is that the rotation speed of the copper rod in step 3 of Comparative Example 2 is 10 m / s, while the rest is the same as in Example 1.
[0038] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that the ball milling process in step 5 of Comparative Example 3 is as follows: 10g of a single grinding ball is added to a ball milling jar for mixing and grinding according to a ball-to-material ratio of 4:1. The alcohol is added until it completely covers the grinding balls and coarse powder. Then the ball mill speed is adjusted to 350r / min and the grinding time is 60min. The alcohol in the ball milling jar is then poured out, and the fine powder floating in the alcohol is screened out.
[0039] Comparative Example 4: The difference between Comparative Example 4 and Example 1 is that in Comparative Example 4, step 2 was not repeatedly melted, but only melted once in each direction. The rest is the same as in Example 1.
[0040] Comparative Examples 5-7: The difference between Comparative Examples 5-7 and Example 1 is that the grain boundary diffusion process of Comparative Examples 5-7 is different, as shown in Table 1. The other processes are the same as those of Example 1.
[0041] Table 1:
[0042] The performance of the high-performance magnets prepared in Examples 1-2 and the magnets prepared in Comparative Examples 1-7 were analyzed, and the results are shown in Table 2 below.
[0043] Table 2:
[0044] Analysis of the data recorded in Table 2 shows that the magnets prepared in Examples 1-2 of this application can achieve the preparation of amorphous diffusion source alloys after optimization of composition and process, and can greatly improve diffusion efficiency, reduce the amount of rare earth elements, and endow the magnets with significant magnetic properties. The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 did not use the binary eutectic composition in NdCu, resulting in a small difference in remanence. However, the coercivity and maximum energy product both showed significant changes, indicating that the binary eutectic composition used in this application helps improve the performance of the magnet. The difference between Comparative Example 2 and Example 1 is that the copper roller rotation speed in Comparative Example 2 was 10 m / s, which significantly reduced both the coercivity and maximum energy product, indicating that the optimization of the copper roller rotation speed in this application also affects the performance of the magnet. The difference between Comparative Example 3 and Example 1 is that the ball milling process was different, resulting in an amorphous powder particle size of 100 μm in Comparative Example 3. Although the remanence increased slightly, the coercivity decreased significantly, indicating that the particle size of the amorphous powder in this application also affects the performance of the magnet. The difference between Comparative Example 4 and Example 1 is that Comparative Example 4 did not undergo repeated melting, but the performance also decreased. The difference between Comparative Examples 5-7 and Example 1 is that the grain boundary diffusion process was different, resulting in significantly different magnet performances. In summary, the combination of the composition and process described in this application can yield high-performance neodymium iron boron magnets.
[0045] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0046] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A method for preparing a high-performance neodymium iron boron magnet, characterized in that, Includes the following steps: Based on the binary or ternary alloy phase diagram of rare earth elements and metals, the eutectic composition of rare earth elements and metals is found. Rare earth element blocks and metal particles are mixed in proportion, and then the rare earth element blocks and metal particles are stacked. The first vacuum is drawn, and the melting process is carried out under the protection of argon atmosphere. After solidification, it is flipped to the other side and melted again. This process is repeated several times. After cooling, the alloy ingot is obtained. The alloy ingot is polished and sheared, then placed in a quartz tube for a second vacuum treatment. Argon gas is then introduced for protection, so that the pressure difference between the furnace body and the outside of the furnace is 0.05 MPa to 0.20 MPa. The rotation speed of the copper roller is adjusted to 25 m / s to 60 m / s. Then, the induction coil heating function is turned on to heat the alloy ingot until it is completely melted. Immediately after that, it is spray-cast to obtain an amorphous alloy strip. The amorphous alloy strip is mechanically crushed and then ground to obtain coarse powder. After the coarse powder is subjected to a first ball milling process, a second ball milling process, and a third ball milling process, it is then dried and sieved to obtain amorphous powder. The amorphous powder, alcohol, and PVB adhesive are mixed evenly to obtain a suspension; The suspension was subjected to ultrasonic vibration and then deposited onto the surface of a magnet. After vacuum drying, the deposited amorphous diffusion source magnet was placed in a hot press furnace with a vacuum degree of 3 × 10⁻⁶. -2 Pa ~ 8×10 -5 Pa, the holding temperature is 400~500℃, and the pressure is 0.5~10 MPa during the period, so that the amorphous diffusion source completes the relaxation behavior under the dual action of amorphous transformation temperature and pressure, which promotes the uniform distribution of the diffusion source on the magnet surface. Then, it diffuses at 900℃~950℃ for 9h~11h, and tempers at 450℃~550℃ for 3h~4h to obtain a high-performance NdFeB magnet.
2. The preparation method according to claim 1, characterized in that, The rare earth element block is one or a mixture of two or more of Dy, Tb, Pr, Nd, Ho, La, Ce, Y, and Sm.
3. The preparation method according to claim 1, characterized in that, The metal particles are one or a mixture of two or more of Al, Cu, Ga, Mg, Zn, Sn, Mn, Co, and Ni.
4. The preparation method according to claim 3, characterized in that, The mass ratio of the rare earth element block to the metal particles is (1.5~9):
1.
5. The preparation method according to claim 1, characterized in that, The vacuum level of the first evacuation was 3 × 10⁻⁶. - 2 Pa ~ 8×10 -5 Pa.
6. The preparation method according to claim 1, characterized in that, The shearing process is 20 × 10 mm. 2 .
7. The preparation method according to claim 1, characterized in that, The vacuum level of the second vacuum pump is 3×10⁻⁶. -2 Pa ~ 8×10 -5 Pa.
8. The preparation method according to claim 1, characterized in that, The first ball milling process involves adding grinding beads with a single bead weight of 8g to 20g to a ball-to-material ratio of 6:1 to 2:1 into a grinding jar for mixing and milling. Alcohol is added until it completely submerges the grinding beads and coarse powder. The ball mill speed is then adjusted to 200 to 350 r / min, and the milling time is 20 to 40 minutes. The alcohol is then poured out of the grinding jar, and the fine powder floating in the alcohol is sieved out. The second ball milling process involves adding alcohol again until it completely submerges the grinding beads and coarse powder. The ball mill speed is adjusted to 200 to 350 r / min, and the milling time is 20 to 40 minutes. The alcohol is then poured out of the grinding jar, and the fine powder floating in the alcohol is sieved out. The third ball milling process involves using grinding beads with a single bead weight of 0.5g to 2g, mixing them in a ball mill jar at a ball-to-material ratio of 6:1 to 2:1, and then adding alcohol again until it completely submerges the grinding beads and coarse powder. The ball mill speed is then adjusted to 200 to 350 r / min. The ball milling speed is 350 r / min to 10 min to 30 min, after which the ball milling beads are removed.
9. The preparation method according to claim 1, characterized in that, The mass ratio of the amorphous powder, alcohol, and PVB adhesive is 1:1:0.
03.
10. The preparation method according to claim 1, characterized in that, The vacuum drying temperature is 10℃~40℃, and the time is 20min~60min.
Citation Information
Patent Citations
Grain boundary diffusion method for improving properties of sintered NdFeB magnets
CN104388951A
Neodymium-iron-boron magnet prepared by utilizing material defects
CN114709040A