Ultra-high performance concrete with large amount of granite saw mud and preparation method thereof

By separating granite sawdust into fine aggregates and activated cementitious materials, and introducing a dual-network hydrogel, the early shrinkage, poor matrix toughness, and construction difficulties of ultra-high performance concrete are solved, thereby improving the utilization rate of sawdust and the performance of concrete.

CN116675489BActive Publication Date: 2024-11-26CHINA STATE CONSTR READY MIXED CONCRETE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310567877.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-26
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

Existing ultra-high performance concrete suffers from problems such as early shrinkage cracking, poor matrix toughness, high construction difficulty and high cost, especially the failure to effectively activate the potential pozzolanic activity of sawdust.

Method used

Granite sawdust was divided into two parts: one part was used as fine aggregate, and the other part was activated and used as an auxiliary cementitious material. A double-network hydrogel was introduced, and the activity of the sawdust was activated by wet ball milling. Hydrogel was prepared by combining inorganic/organic crosslinking to improve the performance of concrete.

Benefits of technology

It improved the utilization rate of sawdust, solved the problems of large early shrinkage, poor matrix toughness and construction difficulties, reduced construction costs and improved the strength and toughness of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004237321200000061
    Figure BDA0004237321200000061
  • Figure BDA0004237321200000071
    Figure BDA0004237321200000071
  • Figure BDA0004237321200000072
    Figure BDA0004237321200000072
Patent Text Reader

Abstract

The present invention belongs to the technical field of building materials, and discloses an ultra-high performance concrete with a large amount of granite saw mud and a preparation method thereof. The ultra-high performance concrete comprises the following raw materials by mass: 70-140 parts of cement, 120-180 parts of unactivated saw mud, 25-50 parts of activated saw mud, 20-45 parts of original fly ash, 20-45 parts of silica fume, 8-20 parts of double network hydrogel with water absorption balance, 1-2 parts of dispersant, 30-50 parts of water, and 2-7 parts of water reducer. The present invention divides the saw mud into two parts, one part is directly used as fine aggregate, and the other part is used as auxiliary cementitious material after activation treatment, which greatly improves the utilization rate of the saw mud; at the same time, the double network hydrogel with water absorption balance is introduced into the concrete, and the effects of its hydrophilic group and hydrophobic group, as well as its shrinkage and water release characteristics and network structure are utilized to solve the problems of large early shrinkage, poor matrix toughness, and difficult construction and maintenance of ultra-high performance concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to ultra-high performance concrete with a large amount of granite saw mud added and a preparation method thereof. Background Art

[0002] With the development of science and technology, the strength grade of concrete has been continuously improved, and ultra-high performance concrete has been successfully applied to civil engineering structures. Ultra-high performance concrete is characterized by low water-binder ratio and sufficient amount of mineral fine admixtures and high-efficiency water reducers, which makes the concrete have comprehensive excellent technical characteristics, but it also produces some performance defects, which limits the application of ultra-high performance concrete in engineering.

[0003] First, many foreign scholars have found that ultra-high performance concrete has the problem of early shrinkage cracking. The reason is that due to the low water-cement ratio and the addition of a large amount of mineral fine admixtures with considerable activity, there is insufficient free water in the micropores of the concrete's internal structure, resulting in insufficient water supply inside the concrete. The internal relative humidity spontaneously decreases and causes self-drying, leading to shrinkage and deformation of the concrete, damaging the internal structure of the concrete and causing microcracks, which have an adverse effect on the structural quality of ultra-high performance concrete.

[0004] Secondly, as the compressive strength of the substrate increases, the problem of poor toughness of the substrate becomes more and more prominent. The compressive strength of ultra-high performance concrete has reached more than 150MPa, but the tensile strength is generally only 1 / 15 to 1 / 20 of the compressive strength, and the ultimate elongation in tension is only 0.005% to 0.05%. At present, steel fiber reinforcement is usually used to improve the toughness of the substrate, but due to the large weight of steel fibers, they are easy to sink to the bottom, and it is difficult to control the distribution of steel fibers inside the matrix, and the toughening effect of steel fibers is difficult to achieve the expected effect.

[0005] Third, ultra-high performance concrete has high requirements for on-site operating conditions. The ultra-high performance concrete slurry caused by factors such as low water-cement ratio and doped steel fiber has excessive viscosity, is difficult to cast and shape, and requires high-temperature curing to achieve the expected strength, which makes construction more difficult and increases construction costs.

[0006] In addition, the high cost of ultra-high performance concrete is also a major factor limiting its engineering application. In order to reduce costs, many studies hope to use solid waste as an admixture in the preparation of concrete. For example, saw mud is often used to partially replace machine-made sand and river sand to optimize the particle grading of fine aggregate, but this method uses a small amount and does not bring out the potential gel activity of saw mud. In fact, the silicon-aluminum compound content of saw mud can reach more than 85%, and it can be used as a cementitious material, but the difficulty lies in how to stimulate its potential volcanic ash activity.

[0007] Therefore, the present invention designs an ultra-high performance concrete with a large amount of granite saw mud, which not only improves the utilization rate of the saw mud, but also solves the defects of the above-mentioned ultra-high performance concrete. Summary of the invention

[0008] The technical problem to be solved by the present invention is to provide an ultra-high performance concrete with a large amount of granite sawn mud and a preparation method thereof in view of the shortcomings of the prior art. The sawn mud is divided into two parts, one part is directly used as fine aggregate, and the other part is used as auxiliary cementitious material after activation treatment, which greatly improves the utilization rate of the sawn mud. At the same time, double-network hydrogel is introduced into the concrete to solve the problems of large early shrinkage, poor matrix toughness and difficult construction and maintenance of ultra-high performance concrete.

[0009] In order to solve the technical problem proposed by the present invention, the present invention provides an ultra-high performance concrete with a large amount of granite saw mud, comprising the following raw materials in parts by weight: 70-140 parts of cement, 120-180 parts of unactivated saw mud, 25-50 parts of activated saw mud, 20-45 parts of original fly ash, 20-45 parts of silica fume, 8-20 parts of double network hydrogel with water absorption balance, 1-2 parts of dispersant, 30-50 parts of water, and 2-7 parts of water reducer.

[0010] In the above scheme, the cement is ordinary Portland cement with a strength grade of 42.5 or 52.5.

[0011] In the above scheme, the moisture content of the original fly ash is 20-30%, SiO 2 The content is 40-50%, Al 2 O 3 The content is 30-40%, the particle size range is 2-200 μm, and the average particle size is 45-52 μm.

[0012] In the above scheme, the specific surface area of ​​the silica fume is 18000-21000m 2 / kg,SiO 2 The content is 90-97%.

[0013] In the above scheme, the dispersant is sodium tripolyphosphate, which increases the dispersion of sawdust in the concrete system.

[0014] In the above scheme, the water reducer is a polycarboxylic acid high-performance water reducer with a solid content of 35-40%.

[0015] In the above scheme, the unactivated saw mud and the activated saw mud are both granite saw mud, and the content of silicon-aluminum compounds thereof is 83-97%, and the water content is ≤3%.

[0016] In the above scheme, the particle size of the unactivated saw mud is 0.6-1.16 mm; the particle size of the activated saw mud is 0.5-1 μm, which is obtained by wet ball milling and then drying the saw mud with a particle size less than 0.6 mm.

[0017] In the above scheme, the preparation method of the activated saw mud is: saw mud, grinding aid, surfactant and water are placed in a ball mill, firstly ground with large grinding balls, then ground with medium and small grinding balls for a second time, and the product is dried to obtain activated saw mud.

[0018] Furthermore, the grinding aid is sodium hexametaphosphate, and the dosage is 0.3-0.5% of the mass of the saw mud.

[0019] Furthermore, the surfactant is sucrose fatty acid ester, and the dosage is 0.03-0.07% of the mass of the saw mud.

[0020] Furthermore, the water dosage controls the water-to-material ratio to be (2-4):1.

[0021] Furthermore, the ball milling equipment is a planetary ball mill, and the matching grinding balls are divided into three sizes: large, medium and small. The particle size of the large grinding balls is 8-10 mm, the particle size of the medium grinding balls is 5-7 mm, and the particle size of the small grinding balls is 2-4 mm.

[0022] Furthermore, the ball-to-material ratio of the primary grinding is 0.5-0.8, and the grinding time is 5-10 minutes.

[0023] Furthermore, the ball-to-material ratio of the secondary grinding is 0.8-1.2, the mass ratio of the small grinding balls to the medium grinding balls is (2-3):1, and the grinding time is 10-15 min.

[0024] Furthermore, the water-to-material ratio is the mass ratio of water to sawdust, and the ball-to-material ratio is the mass ratio of grinding balls to sawdust.

[0025] In the above scheme, the double network hydrogel is a poly (N-isopropylacrylamide) / polyacrylamide inorganic / organic co-crosslinked double network hydrogel, which is polymerized by activated saw mud as an inorganic crosslinker to form a first network structure of poly (N-isopropylacrylamide), and then polymerized by an organic crosslinker in the first network structure to form a second network structure of polyacrylamide.

[0026] In the above scheme, the water absorption rate of the double network hydrogel is 4-5 g / g, the tensile strength is 130-170 KPa, and the elongation at break is 150-300%.

[0027] In the above scheme, the preparation method of the water absorption balanced double network hydrogel is:

[0028] 1) dissolving N-isopropylacrylamide in a first initiator solution, adding activated sawdust and stirring evenly, introducing nitrogen to exhaust air and sealing, performing a first polymerization reaction under constant temperature heating and ultraviolet light conditions, washing and drying the polymer to obtain a first network hydrogel;

[0029] 2) adding acrylamide, an organic crosslinking agent and a silane coupling agent to magnetized water and stirring evenly, then adding the first network hydrogel and the second initiator solution, stirring evenly and then swell in the dark, then introducing nitrogen and exhausting the air, sealing, and performing a second polymerization reaction under ultraviolet light to obtain a double network hydrogel;

[0030] 3) Soaking the double network hydrogel in water to obtain a double network hydrogel with water absorption balance.

[0031] Furthermore, the first initiator solution is a potassium persulfate solution with a concentration of 0.3-0.5 mol / L, and the mass ratio of N-isopropylacrylamide, the first initiator solution and the activated saw mud in step 1) is (2-3):(20-25):1.

[0032] Furthermore, the constant temperature heating temperature of the first polymerization reaction is 40-60° C., the ultraviolet light intensity is 180-240 W, the distance between the ultraviolet light source and the reactants is 25-30 cm, and the reaction time is 1-2 h.

[0033] Furthermore, the cleaning and drying process in step 1) is specifically as follows: the polymer is swelled in water for 2 to 4 hours to remove residual reactants and impurities, and then dried at 45 to 55° C. and 30 to 40% vacuum for 1 to 2 hours.

[0034] Furthermore, the organic crosslinking agent is N,N'-methylenebisacrylamide, the silane coupling agent is KH-570, the magnetized water is water magnetized by a magnetic field of 300-350 mT, and the second initiator solution is a tetramethylammonium hydroxide aqueous solution with a concentration of 20-30%.

[0035] Furthermore, in step 2), the mass ratio of acrylamide, organic crosslinking agent, silane coupling agent, magnetized water, first network hydrogel and second initiator solution is (15-18):1:(1.5-2.5):(110-120):(15-18):(70-80).

[0036] Furthermore, the light-proof swelling time is 8 to 12 hours; the ultraviolet light intensity of the second polymerization reaction is 180 to 240 W, the distance between the ultraviolet light source and the reactants is 25 to 30 cm, and the reaction time is 1 to 2 hours.

[0037] Furthermore, in step 3), the amount of water used is 5 to 10 times the mass of the double network hydrogel, and the soaking time is 30 to 45 minutes.

[0038] The present invention also provides a method for preparing ultra-high performance concrete with a large amount of granite saw mud, comprising the following steps:

[0039] 1) Cement, unactivated sawdust, activated sawdust, original fly ash and silica fume are mixed uniformly to obtain a dry mix;

[0040] 2) adding a water reducing agent, water and a dispersant to the dry mix, mixing evenly, then adding a double network hydrogel with water absorption balance, mixing evenly again, to obtain a mixture;

[0041] 3) The mixture is molded, demoulded and cured after hardening to obtain ultra-high performance concrete with a large amount of granite saw mud.

[0042] In the above scheme, the curing adopts the standard curing conditions of ordinary concrete, with a temperature of 20±2°C and a humidity of more than 95%.

[0043] The main technical concepts of the present invention are as follows:

[0044] 1) In order to improve the utilization rate of saw mud, the present invention divides the saw mud into two parts. The saw mud with a particle size of more than 0.6 mm is directly used as fine aggregate, and the saw mud with a particle size of less than 0.6 mm is activated to serve as an auxiliary cementitious material. The auxiliary cementitious material and the fine aggregate in the concrete base material belong to the same lithology, and the bonding between the component materials inside the matrix is ​​tighter, reducing the interface transition zone, thereby improving the strength of the concrete base material. Saw mud has a high content of silicon-aluminum compounds and has potential volcanic ash activity, but how to effectively stimulate it is a difficult point. Wet ball milling can stimulate the activity of saw mud, but due to the poor uniformity of saw mud particles, simple grinding cannot achieve good results. Therefore, two grindings are adopted. First, large grinding balls are used to impact the saw mud to crush and grind the saw mud with larger particles. As the grinding proceeds, the average particle size of the material continues to decrease, the impact efficiency decreases, and the crushing efficiency gradually increases. At this time, medium and small grinding balls are used in combination. First, the specific surface area of ​​the grinding balls can be increased and the ball milling efficiency can be improved. Second, the combination of grinding balls of different particle sizes can reduce grinding dead angles, making the particle size more uniform and the particle shape more round, thereby maximizing the stimulation of the gel activity of the saw mud.

[0045] 2) In order to solve the problems of large early shrinkage, poor matrix toughness and difficult construction and maintenance of ultra-high performance concrete, the present invention introduces a double network hydrogel. The hydrogel adopts a combination of inorganic / organic crosslinking in the preparation process, and utilizes part of the SiO in the activated saw mud to form a double network hydrogel. 2 The active SiO 2As an inorganic crosslinker of the first network structure, the slight crosslinking with the organic monomer during the polymerization process and the filling effect give the hydrogel excellent strength and toughness. After the hydrogel has absorbed water and reached equilibrium, it is added to the concrete. Since the hydrogel's molecular chain contains hydrophilic groups and hydrophobic groups, a large number of tiny bubbles will be introduced during the mixing process. These bubbles can effectively reduce the friction between the powder particles, thereby increasing fluidity and improving the problem that the ultra-high performance concrete slurry is too viscous and difficult to construct. At the same time, the hydrophilic group will form a hydration film on the surface of the water molecules and the powder particles, which can effectively increase the sliding resistance between the particles, release the free water wrapped by the cement and other particles to participate in the hydration, and reduce the drying shrinkage caused by insufficient free water. In addition, the hydrogel can also use its shrinkage and water release characteristics to achieve the purpose of internal maintenance of ultra-high performance concrete, further reducing the early shrinkage of ultra-high performance concrete. After the water is released, the hydrogel will polymerize into a thin film network structure, and will not leave harmful holes inside the concrete structure system. The additional water in the hydrogel can also continue to react with the unhydrated particles in the ultra-high performance concrete to form a more compact structure. In addition, since the hydrogel has a high tensile strength, the network structure hydrogel retained inside the concrete matrix can effectively enhance the strength and toughness of the concrete matrix.

[0046] In addition, the improvement of the toughness of the ultra-high performance concrete matrix by the hydrogel is mainly due to its long-chain entangled two-component network structure. The first network is a polyelectrolyte rigid structure with strong load-bearing capacity. At the same time, the structural units contain ionizable groups, which have good ionic conductivity and strong dispersion effect, so that the saw mud with a large amount of admixture can be evenly distributed inside the matrix, ensuring the continuity and homogeneity of the material composition inside the structure. The structure as a whole can be evenly stressed to avoid stress concentration. The second network structure is a flexible structure. This layer structure forms multiple cross-linking points with the first network to produce a grid structure. This grid structure can not only effectively divert additional water, but also produce relative slip when the structure is subjected to stress, which can effectively disperse the conducted stress, prevent tip stress concentration, and inhibit the generation and spread of cracks, thereby improving the toughness of the concrete matrix.

[0047] 3) The present invention also uses undisturbed fly ash as raw material. The undisturbed fly ash is low-calcium fly ash that is transported to the ash field and deposited by a hydraulic ash removal system. The undisturbed fly ash after dehydration can be used in construction projects. The use of undisturbed fly ash can greatly improve the utilization rate of fly ash, reduce the grading process of fly ash, and simplify the process. At the same time, the particle size of undisturbed fly ash is large and the particle size distribution is wide. It can supplement the missing particle size in the aggregate and form a compact stacking system with cement, silica fume, activated saw mud and unactivated saw mud, thereby promoting the formation of a dense structure of ultra-high performance concrete.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] The present invention divides sawdust into two parts, one part is used directly as fine aggregate, and the other part is used as auxiliary cementitious material after activation treatment, which greatly improves the utilization rate of sawdust. The present invention also introduces double network hydrogel, which is prepared by combining inorganic / organic crosslinking, has excellent strength and toughness, and is added to concrete after water absorption balance. The effects of its hydrophilic and hydrophobic groups, shrinkage and water release characteristics and network structure are utilized to solve the problems of large early shrinkage, poor matrix toughness and difficult construction and maintenance of ultra-high performance concrete. DETAILED DESCRIPTION

[0050] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0051] In the following examples, the cement used is ordinary Portland cement with a strength grade of 42.5; the moisture content of the original fly ash used is 23%, and the SiO 2 The content is 46%, Al 2 O 3 The content is 33%, the particle size range is 3-144μm, and the average particle size is 48μm; the specific surface area of ​​the silica fume used is 19000m 2 / kg,SiO 2 The content is 96%; the dispersant used is sodium tripolyphosphate; the water reducer used is polycarboxylic acid high-performance water reducer with a solid content of 37%; the unactivated saw mud and the activated saw mud are both granite saw mud, the silicon-aluminum compound content is 87%, and the water content is ≤3%; the particle size range of the granite saw mud is 0.045-1.16mm, the saw mud with a particle size of 0.6-1.16mm is used as the unactivated saw mud, and the saw mud with a particle size of 0.045-0.6mm is wet-milled to a particle size of 0.5-1μm and then dried to use as the activated saw mud.

[0052] Examples 1-4

[0053] The raw material composition and mass fraction of the ultra-high performance concrete with a large amount of granite saw mud in Examples 1-4 are shown in Table 1.

[0054] Table 1 Composition of raw materials of ultra-high performance concrete (unit: parts)

[0055]

[0056] The preparation method of the activated saw mud in Examples 1-4 is as follows (see Table 2 for process parameters):

[0057] Saw mud with a particle size of less than 0.6 mm, sodium hexametaphosphate, sucrose fatty acid ester and water are placed in a planetary ball mill, first ground with large grinding balls, and then ground twice with medium and small grinding balls. The product is dried to obtain activated saw mud; the dosage of sodium hexametaphosphate in Examples 1-4 is 0.3%, 0.35%, 0.4% and 0.5% of the mass of the saw mud, respectively, and the dosage of sucrose fatty acid ester is 0.03%, 0.05%, 0.06% and 0.07% of the mass of the saw mud, respectively.

[0058] Table 2 Wet ball milling process parameters

[0059]

[0060] The preparation method of the double network hydrogel with water absorption balance in Examples 1-4 is:

[0061] 1) dissolving N-isopropylacrylamide in a potassium persulfate solution, adding the activated saw mud and stirring evenly, introducing nitrogen to exhaust the air and sealing, carrying out a first polymerization reaction under constant temperature heating and ultraviolet light conditions (see Table 3 for process parameters), washing and drying the polymer to obtain a first network hydrogel; in Examples 1-4, the mass ratios of N-isopropylacrylamide, potassium persulfate solution and activated saw mud are 2:20:1, 2.3:22:1, 2.7:23:1 and 3:25:1, respectively;

[0062] 2) adding acrylamide, N,N'-methylenebisacrylamide and KH-570 to the magnetized water after the magnetic field and stirring evenly, then adding the first network hydrogel and the tetramethylammonium hydroxide aqueous solution, stirring evenly and then swell in the dark, then introducing nitrogen to exhaust the air and sealing, and performing a second polymerization reaction under ultraviolet light (see Table 4 for process parameters) to obtain a double network hydrogel; in Examples 1-4, the mass ratios of acrylamide, N,N'-methylenebisacrylamide, KH-570, magnetized water, the first network hydrogel and the tetramethylammonium hydroxide aqueous solution are 15:1:1.5:110:15:70, 16:1:1.8:113:16:73, 17:1:2.2:117:76, and 18:1:2.5:120:18:80, respectively;

[0063] 3) Soaking the double network hydrogel in water, wherein the amount of water used in Examples 1-4 is 5, 7, 8, and 10 times the mass of the double network hydrogel, respectively, and the soaking time is 30 min, 35 min, 40 min, and 45 min, respectively, to obtain a double network hydrogel with water absorption balance.

[0064] Table 3 The first polymerization process parameters

[0065]

[0066]

[0067] Table 4 Second polymerization process parameters

[0068]

[0069] The preparation method of the ultra-high performance concrete with a large amount of granite saw mud in Examples 1-4 is as follows:

[0070] 1) Cement, unactivated sawdust, activated sawdust, original fly ash and silica fume are mixed uniformly to obtain a dry mix;

[0071] 2) adding a water reducing agent, water and a dispersant to the dry mix, mixing evenly, then adding a double network hydrogel with water absorption balance, mixing evenly again, to obtain a mixture;

[0072] 3) The mixture is molded, demoulded after hardening, and cured at a temperature of 20±2° C. and a humidity of more than 95% to obtain ultra-high performance concrete with a large amount of granite saw mud.

[0073] Comparative Example 1

[0074] The only difference between Comparative Example 1 and Example 1 is that in the raw material composition of the ultra-high performance concrete, the activated saw mud is replaced by unactivated saw mud, that is, 145 parts of unactivated saw mud and 0 parts of activated saw mud.

[0075] Comparative Example 2

[0076] The difference between Comparative Example 2 and Example 1 is that the preparation method of the activated sawdust adopts only one wet grinding, using grinding balls with a particle size of 10 mm and grinding for 15 minutes.

[0077] Comparative Example 3

[0078] The only difference between Comparative Example 3 and Example 1 is that no water-absorbing balanced double-network hydrogel is added to the raw material composition of the ultra-high performance concrete.

[0079] Comparative Example 4

[0080] The only difference between Comparative Example 4 and Example 1 is that in the raw material composition of the ultra-high performance concrete, the water-absorption-balanced double-network hydrogel is replaced by the water-absorption-balanced single-network polyacrylamide hydrogel.

[0081] The performance of the hydrogel and the ultra-high performance concrete in Examples 1-4 and Comparative Examples 1-4 were tested, wherein the water absorption test method of the hydrogel is as follows: the prepared hydrogel is placed in a beaker and heated, and the hydrogel is discharged until the mass no longer decreases, the mass of the hydrogel is weighed and recorded, and then a certain amount of water is added to the beaker. After standing for a period of time, the hydrogel is taken out, weighed and the mass of the hydrogel is recorded, and the operation is repeated until the mass of the hydrogel after water absorption no longer changes, and its water absorption rate is calculated; the tensile strength and elongation at break of the hydrogel are tested as follows: the hydrogel is trimmed into a cylindrical specimen of Φ2mm×10mm, and the cylindrical specimen is pasted to the upper and lower ends of the testing machine, the prestress is 0.1N, the loading rate is 5mm / min, the load and displacement are recorded when the specimen breaks, the elongation at break is calculated, and the tensile strength is calculated by the cross-sectional area of ​​the specimen. The expansion test of ultra-high performance concrete refers to GB / T 50080-2016 "Test method for performance of ordinary concrete mixtures"; the compressive strength and flexural strength refer to GB / T 50081-2019 "Standard test method for physical and mechanical properties of concrete"; the shrinkage performance test refers to GB / T 50082-2019 "Standard test method for long-term performance and durability of ordinary concrete".

[0082] Table 5 Performance test results

[0083]

[0084] As can be seen from Table 5, in Comparative Example 1, unactivated saw mud was used to prepare ultra-high performance concrete. Since the saw mud was not ground and activated, it lacked activity and did not participate in the hydration reaction. It only played a filling role, which reduced the mechanical properties of the hardened concrete specimen. In Comparative Example 2, saw mud was ground once to activate the saw mud. Compared with the two grindings, the uniformity of the saw mud particles ground once was poor, the grinding was not sufficient, and the activity was not completely stimulated. Therefore, the mechanical properties of the concrete were reduced after hardening. In Comparative Example 3, no hydrogel was added, the free water content was reduced, the fluidity was greatly reduced, and the shrinkage value was significantly increased. After hardening, the concrete matrix lacked the network structure of the double network hydrogel, and the mechanical properties were reduced, among which the flexural strength decreased significantly. In Comparative Example 4, a single network structure polyacrylamide hydrogel was used, and its water absorption, tensile strength, and elongation at break were not as good as those of the double network hydrogel of the present invention. Therefore, the working performance of the mixture was reduced, and the drying shrinkage value of the hardened concrete was also increased due to the reduction of the additional water diversion. The compressive strength and flexural strength of the concrete matrix lacking the double network structure were also reduced.

[0085] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. An ultra-high performance concrete with a large amount of granite saw mud, characterized in that: The method comprises the following raw materials in parts by weight: 70-140 parts of cement, 120-180 parts of unactivated sawdust, 25-50 parts of activated sawdust, 20-45 parts of original fly ash, 20-45 parts of silica fume, 8-20 parts of double network hydrogel with water absorption balance, 1-2 parts of dispersant, 30-50 parts of water, and 2-7 parts of water reducing agent; The particle size of the unactivated saw mud is 0.6-1.16 mm; the particle size of the activated saw mud is 0.5-1 μm. The specific preparation method is: placing saw mud, grinding aid, surfactant and water in a ball mill, first grinding with large grinding balls with a particle size of 8-10 mm, then grinding with medium grinding balls with a particle size of 5-7 mm and small grinding balls with a particle size of 2-4 mm, drying the product to obtain activated saw mud; The double network hydrogel is a poly (N-isopropylacrylamide) / polyacrylamide inorganic / organic co-crosslinked double network hydrogel, which is polymerized by activated sawdust as an inorganic crosslinking agent to form a first network structure of poly (N-isopropylacrylamide), and then polymerized by an organic crosslinking agent in the first network structure to form a second network structure of polyacrylamide.

2. The ultra-high performance concrete with a large amount of granite saw mud according to claim 1 is characterized in that: The unactivated saw mud and the activated saw mud are both granite saw mud, with a silicon-aluminum compound content of 83-97% and a moisture content of ≤3%; the original fly ash has a moisture content of 20-30%, a SiO2 content of 40-50%, an Al2O3 content of 30-40%, a particle size range of 2-200 μm, and an average particle size of 45-52 μm.

3. The ultra-high performance concrete with a large amount of granite saw mud according to claim 1, characterized in that: The ball milling equipment is a planetary ball mill; the ball-to-material ratio of the primary grinding is 0.5-0.8, and the grinding time is 5-10 minutes; the ball-to-material ratio of the secondary grinding is 0.8-1.2, the mass ratio of small grinding balls to medium grinding balls is (2-3):1, and the grinding time is 10-15 minutes.

4. The ultra-high performance concrete with a large amount of granite saw mud according to claim 1, characterized in that: The double network hydrogel has a water absorption rate of 4-5 g / g, a tensile strength of 130-170 KPa, and an elongation at break of 150-300%.

5. The ultra-high performance concrete with a large amount of granite saw mud according to claim 1, characterized in that: The preparation method of the double network hydrogel with water absorption balance is as follows: 1) dissolving N-isopropylacrylamide in a first initiator solution, adding activated sawdust and stirring evenly, introducing nitrogen to exhaust air and sealing, performing a first polymerization reaction under constant temperature heating and ultraviolet light conditions, washing and drying the polymer to obtain a first network hydrogel; 2) adding acrylamide, an organic crosslinking agent and a silane coupling agent to magnetized water and stirring evenly, then adding the first network hydrogel and the second initiator solution, stirring evenly and swelling in the dark, then introducing nitrogen gas to expel the air and sealing, and performing a second polymerization reaction under ultraviolet light to obtain a double network hydrogel; 3) Soaking the double network hydrogel in water to obtain a double network hydrogel with water absorption balance.

6. The ultra-high performance concrete with a large amount of granite saw mud according to claim 5, characterized in that: In step 1), the mass ratio of N-isopropylacrylamide, the first initiator solution and the activated saw mud is (2-3): (20-25): 1; in step 2), the mass ratio of acrylamide, the organic crosslinking agent, the silane coupling agent, the magnetized water, the first network hydrogel and the second initiator solution is (15-18): 1: (1.5-2.5): (110-120): (15-18): (70-80).

7. The ultra-high performance concrete with a large amount of granite saw mud according to claim 5, characterized in that: The constant temperature heating temperature of the first polymerization reaction is 40-60° C.; the UV light intensity of the first polymerization reaction and the second polymerization reaction is 180-240 W, the distance between the UV light source and the reactants is 25-30 cm, and the reaction time is 1-2 h.

8. A method for preparing ultra-high performance concrete with a large amount of granite saw mud as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: 1) Take cement, unactivated sawdust, activated sawdust, original fly ash and silica fume, mix them evenly to obtain a dry mix; 2) adding a water reducing agent, water and a dispersant to the dry mix, mixing evenly, then adding the double network hydrogel with water absorption balance, mixing evenly again, and obtaining a mixture; 3) The mixture is molded, demoulded and cured after hardening to obtain ultra-high performance concrete with a large amount of granite saw mud.

9. The method for preparing ultra-high performance concrete with a large amount of granite saw mud according to claim 8, characterized in that: The curing temperature is 20±2°C and the humidity is above 95%.