A multi-level porous boron carbon nitrogen material and its preparation method and application

By using carbon balls as hard templates and carbon sources in the oxidative desulfurization system, hierarchical porous boron carbon nitride materials are prepared, which solves the problem of insufficient activity of existing boron nitride materials and achieves ultra-deep desulfurization of aromatic sulfides in diesel. And the controllability of the catalyst is improved, which significantly improves the catalytic performance and the convenience of recycling.

CN116689014BActive Publication Date: 2024-10-25JIANGSU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310881359.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-18
Publication Date
2024-10-25
Estimated Expiration
2043-07-18

AI Technical Summary

Technical Problem

Existing boron nitride materials have limited oxidation activity for aromatic sulfides in oxidative desulfurization systems and cannot achieve the goal of ultra-deep desulfurization. Moreover, the synthesis of boron carbon nitride materials has poor controllability and low catalytic active site content.

Method used

Carbon spheres are used as hard templates and carbon sources, hydrophilic carbon spheres are prepared through hydrothermal reaction, and are calcined at high temperature in the presence of ammonia gas to synthesize hierarchical porous boron carbon nitrogen materials to build microporous, mesoporous and macroporous structures. , improve the concentration of catalytic active sites and oxidative desulfurization performance.

Benefits of technology

Ultra-deep desulfurization of aromatic sulfides in diesel is achieved. The controllability and active site concentration of the catalyst are significantly improved, the mass transfer efficiency is enhanced, and the catalytic performance is optimized. Ultra-deep desulfurization (<10ppm) can be achieved and the circulation of the catalyst can be improved. Ease of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116689014B_ABST
    Figure CN116689014B_ABST
Patent Text Reader

Abstract

The present invention discloses a multi-level porous boron carbon nitrogen material and its preparation method and application. Hydrophilic carbon balls of different sizes are used as hard templates and carbon sources, boric acid, boron oxide, etc. are used as boron sources, urea, thiourea, melamine, etc. are used as nitrogen sources, and the precursor is synthesized by a dispersion dissolution recrystallization method. By pyrolyzing the precursor, a large number of gas small molecules generated by high-temperature pyrolysis are used to form micropores, and mesopores or macropores are constructed using the carbon ball hard template, and finally a multi-level porous boron carbon nitrogen is formed. The microporous structure of the multi-level porous boron carbon nitrogen catalyst prepared by the present invention can have a large number of defect sites, which can increase the concentration of catalytic active sites of the boron carbon nitrogen material; the macropore and mesoporous structure can enhance the mass transfer efficiency during the catalytic reaction. The prepared multi-level porous boron carbon nitrogen material is used for activated oxygen diesel oxidation desulfurization, which can achieve ultra-deep desulfurization of diesel, and can directionally convert dibenzothiophene aromatic sulfides into high-value-added sulfones.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional catalytic material preparation and catalysis, and specifically relates to a multi-level porous boron carbon nitrogen material and a preparation method thereof and application thereof in catalytic oxidation desulfurization of fuel oil. Background Art

[0002] In recent years, due to the increase in the consumption of fossil fuels such as diesel, the pollution problem caused by the combustion of sulfides therein has become increasingly serious. The emission of sulfur oxides (SOx) can lead to pollution problems such as acid rain and haze. Therefore, many countries and regions have formulated increasingly stringent regulations to limit the sulfur content in fuel to 10ppm or less. Generally, hydrodesulfurization (HDS) is the most commonly used desulfurization technology in industry. Studies have found that HDS has a high efficiency in removing aliphatic sulfides. However, due to the aromaticity and steric hindrance of aromatic sulfides, HDS has low activity towards aromatic sulfides such as dibenzothiophene and its derivatives. Researchers have found that oxidative desulfurization has attracted widespread attention due to its advantages such as high activity, low cost and mild reaction conditions for aromatic sulfides. In particular, due to the O 2 Oxygen (O 2 ) as the oxidant has attracted much attention. Designing a highly active catalyst is the key to achieving the goal of using O 2 It is the key to oxidative desulfurization.

[0003] Boron nitride materials are widely used in the field of catalysis due to their high specific surface area, good thermal and chemical stability, structural designability and other advantages, such as catalytic propane dehydrogenation (Science, 2016, 354, 1570-1573), oxidative desulfurization (Small, 2017, 13, 1701857), etc. However, the applicant found in the previous research work that in the oxidative desulfurization system, the oxidation activity of commercial-grade BN on sulfides is limited, far from achieving the goal of ultra-deep desulfurization (Green Energy & Environment, 2020, 5, 166-172), so it is necessary to modify the boron nitride material to improve its catalytic oxidative desulfurization performance.

[0004] Among them, the study found that carbon atom doping to construct boron carbon nitrogen materials is a strategy that can significantly improve their catalytic activity. By doping with carbon atoms, the charge structure of the catalytic active sites can be regulated, significantly improving the O 2 The activation ability of O 2Catalytic oxidative desulfurization activity (Microporous and Mesoporous Materials, 2020, 293, 109788). However, the synthesis of boron carbon nitrogen materials is usually synthesized by introducing carbon-containing organic precursors for thermal decomposition, which has poor controllability and difficulty in adjusting the pore structure, resulting in a low content of catalytic active sites and poor performance in activating O 2 The oxidative desulfurization has deficiencies such as obstructed mass transfer. Summary of the invention

[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a method for controlling the preparation of multi-level porous boron carbon nitrogen materials by using carbon spheres as hard templates and carbon sources in view of the deficiencies in the prior art.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing a multi-level porous boron carbon nitrogen material comprises the following steps:

[0008] (1) Preparation of hydrophilic carbon spheres;

[0009] (2) mixing and uniformly dispersing the hydrophilic carbon spheres, the boron source, and the nitrogen source in water, and then stirring under an oil bath until the water is completely evaporated to obtain a gray-black solid;

[0010] (3) calcining the gray-black solid obtained in step (2) at high temperature in the presence of ammonia gas, and naturally cooling to room temperature after calcination to obtain the product.

[0011] Specifically, in step (1), the hydrophilic carbon spheres are prepared using glucose or water-soluble cellulose as raw materials through a hydrothermal reaction, specifically, the raw materials are dissolved in water, then transferred to a reactor, and subjected to a hydrothermal reaction at 160-200°C (preferably 160-180°C) for 6-18h (preferably 12-16h). After the reaction is completed, the mixture is naturally cooled to room temperature, the carbon spheres are separated by centrifugation, and washed alternately with water and ethanol, and dried to obtain hydrophilic carbon spheres of different sizes.

[0012] Specifically, the dosage ratio of raw materials to water is (0.5-5.0 g): (50-80 mL), preferably (1.0-3.0 g): (50-60 mL); the hydrothermal reaction temperature is 160-180° C., and the hydrothermal time is 12-16 h; the centrifugal separation speed is 6000-10000 rpm, preferably 8000-10000 rpm; the centrifugal time is 3-10 min, preferably 5-8 min; the volume of water during washing is 10-50 mL, preferably 20-40 mL; the volume of ethanol is 10-50 mL, preferably 20-40 mL; and the drying temperature is 80-160° C., preferably 100-120° C.

[0013] Specifically, in step (2), the boron source is any one of boric acid, boric oxide, borax, or a mixture of two or more thereof, preferably boric acid; the nitrogen source is any one of urea, melamine, dicyandiamide, thiourea, or a mixture of two or more thereof, preferably urea and thiourea.

[0014] Specifically, in step (2), the mass ratio of the boron source to the nitrogen source is 1:10-1:50, preferably 1:20-1:40; the mass ratio of the hydrophilic carbon spheres to the boron source is 1:10-1:50, preferably 1:20-1:40.

[0015] Specifically, in step (2), the temperature of the oil bath is controlled at 60-110° C., preferably 80-100° C.; magnetic stirring is used for stirring, and the rotation speed is 100-1200 rpm, preferably 600-800 rpm.

[0016] Specifically, in step (3), the gray-black solid is transferred to an ark and then placed in a tubular furnace for high-temperature calcination; the ark is made of ceramic, quartz or corundum, preferably quartz; the furnace tube in the tubular furnace is made of ceramic, quartz or corundum, preferably quartz; the high-temperature calcination temperature is 800-1200°C, preferably 800-1000°C; the holding time is 2-8h, preferably 4-6h; the heating rate of the tubular furnace is 1-10°C / min, preferably 5-8°C / min; the calcination atmosphere is ammonia or a mixture of ammonia and nitrogen, preferably a mixture of ammonia and nitrogen, the mixing ratio of ammonia to nitrogen is 20:80-80:20, preferably 50:50; the gas flow rate is 50-200mL / min, preferably 100mL / min.

[0017] Furthermore, the multi-level porous boron carbon nitrogen material prepared by the above preparation method is also within the protection scope of the present invention.

[0018] Furthermore, the multi-level porous boron carbon nitrogen material prepared by the present invention is composed of three elements: boron, carbon and nitrogen, and has at least two structures of micropores, mesopores and macropores; wherein the micropore size is 0.1-1.8nm, preferably 0.2-1nm; the mesopore size is 10-50nm, preferably 20-40nm; the macropore size is 60-200nm, preferably 80-120nm.

[0019] The preparation principle of the present invention is as follows:

[0020] Carbon spheres decompose when calcined at high temperature in the presence of ammonia, and can be used as hard templates to synthesize macroporous or mesoporous hard templates. At the same time, carbon spheres can also be used as carbon sources for the synthesis of boron carbon nitrogen materials. In addition, a large amount of gas will be produced during the reaction of the boron source and the nitrogen source, and a large amount of gas small molecules will also be produced during the decomposition of the carbon spheres, which can construct a large number of micropores and increase the concentration of catalytic active sites. The present invention uses hydrophilic carbon spheres as hard templates and carbon sources, and utilizes the characteristics of high-temperature decomposition of carbon spheres in the presence of ammonia as hard templates to construct macroporous or mesoporous structures; and utilizes the gas small molecules generated by the decomposition of carbon spheres and the decomposition of boron sources and nitrogen sources to construct microporous structures. The prepared multi-level porous boron carbon nitrogen material has both microporous and mesoporous structures, or has both microporous and macroporous structures, or has both microporous, mesoporous and macroporous structures. Therefore, the multi-level porous boron carbon nitrogen material of the present invention not only has a rich microporous structure to improve catalytic activity, but also has an ordered mesoporous or macroporous structure, which strengthens the activation of O 2 Mass transfer efficiency of the oxidative desulfurization process.

[0021] Furthermore, the present invention also claims that the multi-level porous boron carbon nitrogen material is activated by O 2 Application in catalytic fuel oxidation to remove aromatic sulfides. It can achieve ultra-deep desulfurization of fuels such as diesel, and achieve directional conversion of sulfides into sulfones.

[0022] Preferably, the aromatic sulfide is a dibenzothiophene aromatic sulfide.

[0023] Preferably, the amount of the multi-level porous boron carbon nitrogen catalyst added is 0.5-1.0 g per 100 mL of diesel.

[0024] The multi-level porous boron carbon nitrogen catalyst is premixed with diesel, and then oxygen is introduced as an oxidant, heated in a constant temperature oil bath, and magnetically stirred, and a small amount of supernatant is taken out regularly for analysis by gas chromatography to determine the remaining sulfur content in the oil. Among them, the amount of multi-level porous boron carbon nitrogen catalyst added is 0.5-1.0g per 100mL model oil, the initial sulfide concentration in the model oil is 10-500ppmw, the oxygen pressure is 0.1MPa, the oxygen flow rate is 20-200mL / min, the reaction temperature is 100-150℃, the reaction time is 2-8h, the magnetic stirring rate is 600-1200rpm, and the desulfurization product obtained is the corresponding sulfone.

[0025] The model oils include dibenzothiophene (DBT) model oil, 4,6-dimethyldibenzothiophene (4,6-DMDBT) model oil and 4-methyldibenzothiophene (4-MDBT), among which the oxidation removal effect of 4,6-DMDBT is the best.

[0026] When the desulfurization temperature is 120°C, the oxidation desulfurization performance is the best.

[0027] When the magnetic stirring speed is 1000 rpm, the oxidation desulfurization performance is the best, that is, deep desulfurization can be achieved.

[0028] When the oxygen flow rate is 100 mL / min, both the oil yield and the desulfurization rate can be achieved.

[0029] The desulfurization product sulfone refers to dibenzothiophene sulfone, 4,6-dimethyldibenzothiophene sulfone and 4-methyldibenzothiophene sulfone, which has high economic added value and can improve the economy of the desulfurization process.

[0030] Beneficial effects:

[0031] (1) The present invention uses hydrophilic carbon spheres as hard templates and carbon sources to construct a multi-level porous boron carbon nitrogen material to achieve charge regulation of catalytic active sites. At the same time, the micropores of the multi-level pores can construct a richer active site concentration, and the mesoporous or macroporous structure enhances the transfer and diffusion of substrate molecules in the desulfurization process, thereby improving the desulfurization efficiency.

[0032] (2) The multi-level porous boron carbon nitrogen material prepared by the process route proposed in the present invention has a better controllable pore structure than the boron carbon nitrogen material synthesized by the traditional soft template, and can improve the catalytic performance and concentration of the catalytic active sites, and enhance the activation of O 2 Catalyzes diesel oxidation desulfurization to achieve ultra-deep desulfurization of diesel (<10ppm).

[0033] (3) The multi-level porous boron carbon nitrogen material constructed by the present invention is a multiphase catalyst that can be efficiently separated from diesel, realize the recovery and regeneration of the catalyst after the desulfurization reaction, and improve the convenience of catalyst recycling.

[0034] (4) The oxidant used in the present invention is O 2 , widely available and inexpensive; at the same time, no other solvents need to be added during the reaction, which is green, environmentally friendly and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0036] Figure 1 The electron microscope and pore size distribution diagram of the multi-level porous boron carbon nitride prepared in Example 1. Among them, a is the SEM image of the multi-level porous boron carbon nitride material, b is the TEM image of the multi-level porous boron carbon nitride material, c is the nitrogen adsorption and desorption isotherm diagram of the multi-level porous boron carbon nitride material; d is the pore size distribution diagram of the multi-level porous boron carbon nitride material response.

[0037] Figure 2: It is the electron microscope and pore size distribution diagram of the multi-level porous boron carbon nitride material prepared in Example 2. Among them, a is the SEM image of the multi-level porous boron carbon nitride material, b is the TEM image of the multi-level porous boron carbon nitride material, c is the nitrogen adsorption and desorption isotherm diagram of the multi-level porous boron carbon nitride material; d is the pore size distribution diagram of the multi-level porous boron carbon nitride material response.

[0038] Figure 3 This is a transmission electron microscope image of the multi-level porous boron carbon nitride material prepared in Example 3.

[0039] Figure 4 This is a transmission electron microscope image of the multi-level porous boron carbon nitride material prepared in Example 4.

[0040] Figure 5 This is a transmission electron microscope image of the multi-level porous boron carbon nitride material prepared in Example 5.

[0041] Figure 6 It is a hierarchical porous boron carbon nitrogen material catalyst used to activate O 2 Data on the effectiveness of oxidative removal of aromatic sulfides from diesel.

[0042] Figure 7 This is a transmission electron microscope image of the boron carbon nitride material prepared in Comparative Example 1.

[0043] Figure 8 This is a transmission electron microscope image of the boron carbon nitride material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0044] The present invention can be better understood with reference to the following examples.

[0045] Embodiment 1:

[0046] (1) Dissolve 2.0 g of glucose in 50 mL of deionized water, then transfer to a 100 mL hydrothermal reactor, heat at 180 ° C for 12 h, and cool naturally to room temperature. Then centrifuge in a high-speed centrifuge at 8000 rpm for 5 min. Wash the obtained white solid three times with 20 mL of water, then wash three times with 20 mL of ethanol, and dry at 100 ° C.

[0047] (2) Boric acid and urea (mass ratio of 1:20) were dissolved in deionized water, and then the carbon spheres (mass ratio of carbon spheres to boric acid was 1:20) were added, and then transferred to a constant temperature oil bath, heated and stirred at 80°C, with a stirring speed of 800 rpm, until the solvent was completely evaporated to obtain an off-white solid.

[0048] (3) The off-white solid obtained in step (2) was transferred to a quartz ark, and the quartz ark was placed in a tubular furnace made of quartz tube material, and a mixture of ammonia and nitrogen in a ratio of 50:50 was introduced, and the gas flow rate was 100 mL / min, and the temperature was increased to 900°C at a heating rate of 5°C / min, and maintained for 4 hours, and then naturally cooled to room temperature to obtain a multi-level porous boron carbon nitrogen material. The scanning electron microscope (SEM) and transmission electron microscope (TEM) are as follows: Figure 1 As shown. Figure 1 From the SEM image of a, it can be seen that the synthesized boron carbon nitrogen material is assembled from two-dimensional thin-layer nanosheets, and the existence of pores can be observed; further Figure 1 As can be seen from the TEM image b, with the hydrophilic carbon sphere as the hard template, an ordered mesoporous structure can be seen, and the size of the mesopores is 25-35nm. Since the size of the micropores cannot be observed in the TEM image, the obtained sample was further subjected to nitrogen adsorption and desorption isothermal analysis. Figure 1 It can be seen from the nitrogen adsorption-desorption curve of c that there is an obvious rise in the low partial pressure region, indicating the existence of a large number of microporous structures, and there is an H3 type hysteresis loop in the range of 0.4 to 1.0, indicating the existence of mesopores. Figure 1 It can be seen from the pore size distribution of d that the obtained sample contains particles with a size of about The micropores and of mesopores.

[0049] Embodiment 2:

[0050] (1) Dissolve 1.0 g of glucose in 60 mL of deionized water, then transfer to a 100 mL hydrothermal reactor, heat at 160 ° C for 18 h, and cool naturally to room temperature. Then centrifuge in a high-speed centrifuge at 10,000 rpm for 7 min. Wash the obtained white solid three times with 30 mL of water, then wash three times with 30 mL of ethanol, and dry at 100 ° C.

[0051] (2) Boric acid and urea (mass ratio of 1:30) were dissolved in deionized water, and then the carbon spheres (mass ratio of carbon spheres to boric acid was 1:30) were added, and then transferred to a constant temperature oil bath, heated and stirred at 90° C., with a stirring speed of 900 rpm, until the solvent was completely evaporated to obtain an off-white solid.

[0052] (3) The off-white solid obtained in step (2) was transferred to a quartz ark, and the quartz ark was placed in a tubular furnace made of quartz tube material, and a mixture of 50:50 ammonia and nitrogen was introduced at a gas flow rate of 120 mL / min, and the temperature was increased to 1000°C at a heating rate of 4°C / min, maintained for 3 hours, and then naturally cooled to room temperature to obtain a multi-level porous boron carbon nitrogen material. Its nitrogen adsorption and desorption isotherms and pore size distribution are shown in FIG. Figure 2 As shown. Figure 2 The SEM image of a shows that the synthesized boron carbon nitrogen material is assembled from two-dimensional thin-layer nanosheets, and has a fluffy structure due to the presence of micropores and mesopores. Figure 2 As can be seen from the TEM image b, with the hydrophilic carbon sphere as the hard template, an ordered mesoporous structure can be seen, and the size of the mesopores is Since the micropore size cannot be observed in the TEM image, the obtained sample was further subjected to nitrogen adsorption and desorption isothermal analysis. Figure 2 c It can be seen from the nitrogen adsorption-desorption curve of the sample that the adsorption amount suddenly increases in the low relative pressure range, indicating the existence of a large number of microporous structures, and there is an H3 type hysteresis curve in the range of 0.4 to 1.0, indicating the existence of mesoporous structures in the sample. It can also be seen from the pore size distribution curve calculated using the adsorption branch data that Figure 2 As shown in d, there are a large number of microporous mesoporous structures, and the pore size is about 4

[0053] Embodiment 3:

[0054] (1) Dissolve 2.0 g of glucose in 50 mL of deionized water, then transfer to a 100 mL hydrothermal reactor, heat at 180 ° C for 12 h, and cool naturally to room temperature. Then centrifuge in a high-speed centrifuge at 8000 rpm for 5 min. Wash the obtained white solid three times with 20 mL of water, then wash three times with 20 mL of ethanol, and dry at 100 ° C.

[0055] (2) Boric acid and urea (mass ratio of 1:20) were dissolved in deionized water, and then the carbon spheres (mass ratio of carbon spheres to boric acid was 1:20) were added, and then transferred to a constant temperature oil bath, heated and stirred at 80°C, with a stirring speed of 800 rpm, until the solvent was completely evaporated to obtain an off-white solid.

[0056] (3) The off-white solid obtained in step (2) is transferred to a quartz ark, and the quartz ark is placed in a tubular furnace made of quartz tube material, and a mixture of 50:50 ammonia and nitrogen is introduced, the gas flow rate is 100 mL / min, and the temperature is increased to 1100°C at a heating rate of 2°C / min, maintained for 4 hours, and then naturally cooled to room temperature to obtain a multi-level porous boron carbon nitrogen material. Figure 3 It can be seen that since the same carbon spheres as in Example 1 were used as templates, the morphology of the obtained porous boron carbon nitrogen material was similar to that in Example 1, indicating that porous boron carbon nitrogen material can also be synthesized at 1100°C, and the pore structure is mainly determined by the hydrophilic carbon sphere template, rather than the calcination temperature.

[0057] Embodiment 4:

[0058] (1) Dissolve 1.0 g of glucose in 60 mL of deionized water, then transfer to a 100 mL hydrothermal reactor, heat at 160 ° C for 18 h, and cool naturally to room temperature. Then centrifuge in a high-speed centrifuge at 10,000 rpm for 7 min. Wash the obtained white solid three times with 30 mL of water, then wash three times with 30 mL of ethanol, and dry at 100 ° C.

[0059] (2) Boric acid and urea (mass ratio of 1:30) were dissolved in deionized water, and then the carbon spheres (mass ratio of carbon spheres to boric acid was 1:30) were added, and then transferred to a constant temperature oil bath, heated and stirred at 90° C., with a stirring speed of 900 rpm, until the solvent was completely evaporated to obtain an off-white solid.

[0060] (3) The off-white solid obtained in step (2) is transferred to a quartz ark, and the quartz ark is placed in a tubular furnace made of quartz tube material, and a mixture of 50:50 ammonia and nitrogen is introduced, the gas flow rate is 120 mL / min, and the temperature is increased to 800°C at a heating rate of 5°C / min, maintained for 3 hours, and then naturally cooled to room temperature to obtain a multi-level porous boron carbon nitrogen material. Figure 4 It can be seen that since the same carbon spheres as in Example 2 were used as templates, the morphology of the obtained porous boron carbon nitrogen material was similar to that in Example 2, indicating that porous boron carbon nitrogen material can also be synthesized at 800°C, and the pore structure is mainly determined by the hydrophilic carbon sphere template, rather than the calcination temperature.

[0061] Example 5

[0062] (1) 0.5 g of water-soluble cellulose was dissolved in 50 mL of deionized water, then transferred to a 100 mL hydrothermal reactor, hydrothermally heated at 180°C for 12 h, and naturally cooled to room temperature. The mixture was then centrifuged in a high-speed centrifuge at 8000 rpm for 5 min. The obtained white solid was washed three times with 20 mL of water, then washed three times with 20 mL of ethanol, and dried at 100°C.

[0063] (2) Boric acid and urea (mass ratio of 1:20) were dissolved in deionized water, and then the carbon spheres (mass ratio of carbon spheres to boric acid was 1:20) were added, and then transferred to a constant temperature oil bath, heated and stirred at 80°C, with a stirring speed of 800 rpm, until the solvent was completely evaporated to obtain an off-white solid.

[0064] (3) The off-white solid obtained in step (2) was transferred to a quartz ark, and the quartz ark was placed in a tubular furnace made of quartz tube material, and a mixture of 50:50 ammonia and nitrogen was introduced, and the gas flow rate was 100 mL / min, and the temperature was increased to 900°C at a heating rate of 5°C / min, and maintained for 4 hours, and then naturally cooled to room temperature to obtain a multi-level porous boron carbon nitrogen material. Its transmission electron microscopy (TEM) is as follows Figure 5 As shown in the TEM image, it can be seen that with the hydrophilic carbon sphere as the hard template, a large number of micropores can be seen, and the pore size is about 1.5nm. At the same time, a large number of ordered mesopores can be observed, and the mesopore size is about 50nm.

[0065] Embodiment 6-13

[0066] The multi-level porous boron carbon nitrogen material catalyst obtained in Example 1-2 was used to activate O 2 Oxidative removal of aromatic sulfides in diesel. The following are the types of simulated diesel oil and the composition of the oxidative desulfurization experimental device:

[0067] The preparation process of the model oil is as follows: DBT, 4,6-DMDBT, and 4-MDBT are respectively dissolved in dodecane to prepare a model oil with a sulfide concentration of 10-500 ppmw, and n-tetradecane is added as an internal standard.

[0068] Add model oil to a round-bottom flask, then add a certain amount of the multi-level porous boron carbon nitrogen catalyst obtained in Example 1 or Example 2, and premix with the model oil, then introduce oxygen as an oxidant, heat in a constant temperature oil bath, and stir magnetically, take out a small amount of supernatant regularly for analysis by gas chromatography, determine the remaining sulfur content in the oil, and analyze the obtained desulfurization product by GC-MS. The desulfurization rate calculation formula is as follows:

[0069]

[0070] The experimental results of the embodiment are as follows Figure 6 As shown, it can be seen that the multi-level porous boron carbon nitrogen material synthesized by the present invention can indeed efficiently remove aromatic sulfides, and the removal effect is good. For different sulfides, under the optimized reaction conditions of the present application, a desulfurization rate of >98% can be achieved, and it can be directed into sulfone.

[0071] Comparative Example 1

[0072] (1) Literature reports that after carbon materials are subjected to high temperatures, most of the oxygen-containing groups on the surface of the carbon materials will be eliminated, showing hydrophobicity (Journal of Inorganic Chemistry, 2022, 38, 1-13). Therefore, the carbon spheres obtained in Example 1 were treated at 900°C under nitrogen protection to obtain hydrophobic carbon spheres.

[0073] (2) Boric acid and urea (mass ratio of 1:20) were dissolved in deionized water, and then the carbon spheres (mass ratio of carbon spheres to boric acid was 1:20) were added, and then transferred to a constant temperature oil bath, heated and stirred at 80°C, with a stirring speed of 800 rpm, until the solvent was completely evaporated to obtain an off-white solid.

[0074] (3) The off-white solid obtained in step (2) was transferred to a quartz ark, and the quartz ark was placed in a tubular furnace made of quartz tube material, and a mixture of 50:50 ammonia and nitrogen was introduced, and the gas flow rate was 100 mL / min, and the temperature was increased to 900°C at a heating rate of 5°C / min, maintained for 4 hours, and then naturally cooled to room temperature to obtain a boron carbon nitrogen material. The morphology results are as follows Figure 7 As shown, due to the hydrophobicity of carbon spheres, carbon spheres cannot be highly dispersed in the precursor. Therefore, the obtained boron carbon nitrogen material has no obvious pore structure and no obvious ordered structure.

[0075] (4) The boron carbon nitrogen material obtained above was used to remove DBT from model diesel according to the conditions of Example 6. Since it does not contain a porous structure, its active site exposure is low and the mass transfer efficiency of the reaction process is low, and its desulfurization rate is only 70%.

[0076] Comparative Example 2

[0077] (1) Literature reports that organic matter can also be used as a carbon source to synthesize boron carbon nitrogen materials (Angew. Chem. Int. Ed. 2018, 57, 5487.). Therefore, as a control sample, the applicant selected glucose as a carbon source to synthesize boron carbon nitrogen materials.

[0078] (2) Boric acid and urea (mass ratio of 1:20) were dissolved in deionized water, and then the carbon spheres were added (the mass ratio of carbon in glucose to boric acid was controlled to be 1:20), and then transferred to a constant temperature oil bath, heated and stirred at 80°C at a stirring speed of 800 rpm until the solvent was completely evaporated to obtain an off-white solid.

[0079] (3) The off-white solid obtained in step (2) was transferred to a quartz ark, and the quartz ark was placed in a tubular furnace made of quartz tube material, and a mixture of 50:50 ammonia and nitrogen was introduced, and the gas flow rate was 100 mL / min, and the temperature was increased to 900°C at a heating rate of 5°C / min, maintained for 4 hours, and then naturally cooled to room temperature to obtain a boron carbon nitrogen material. The morphology results are as follows Figure 8 As shown. Since glucose, as a carbon source, cannot serve as a hard template, it cannot form an ordered pore structure. Only micropores created by the precursor and the gas produced by the decomposition of glucose exist, making it only present as a layered structure of a two-dimensional material.

[0080] (4) The boron carbon nitrogen material obtained above was used to remove DBT from model diesel according to the conditions of Example 6. Since it only contained micropores but no ordered mesopores or macropores, the mass transfer efficiency of the reaction process was low and the desulfurization rate was only 80%.

[0081] The present invention provides a multi-level porous boron carbon nitrogen material and its preparation method and application ideas and methods. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.

Claims

1. A method for preparing a multi-level porous boron carbon nitrogen material, characterized in that: The steps include: (1) Preparation of hydrophilic carbon spheres; (2) mixing the hydrophilic carbon spheres, the boron source, and the nitrogen source and uniformly dispersing them in water, and then stirring them under an oil bath until the water is completely evaporated to obtain an off-white solid; (3) calcining the off-white solid obtained in step (2) at high temperature in a mixed gas of ammonia and nitrogen, and cooling naturally to room temperature after calcination to obtain; In step (1), the hydrophilic carbon spheres are prepared by hydrothermal reaction using glucose or water-soluble cellulose as raw materials, specifically, the raw materials are dissolved in water, and then transferred to a reactor for hydrothermal reaction, and naturally cooled to room temperature after the reaction, and the carbon spheres are separated by centrifugation, and then washed alternately with water and ethanol, and dried to obtain hydrophilic carbon spheres of different sizes; The dosage ratio of raw materials to water is (0.5-5.0 g): (50-80 mL); the hydrothermal reaction temperature is 160-180°C, and the hydrothermal time is 12-16 h; the centrifugal separation speed is 6000-10000 rpm, and the centrifugal time is 3-10 min; the drying temperature is 80-160°C; In step (2), the boron source is any one of boric acid, boric oxide, and borax, or a mixture of two or more thereof; the nitrogen source is any one of urea, melamine, dicyandiamide, and thiourea, or a mixture of two or more thereof; The mass ratio of the boron source to the nitrogen source is 1:10-1:50, and the mass ratio of the hydrophilic carbon sphere to the boron source is 1:10-1:

50.

2. The method for preparing the multi-level porous boron carbon nitrogen material according to claim 1, characterized in that: In step (2), the temperature of the oil bath is controlled at 60-110° C., and the stirring is performed by magnetic stirring at a rotation speed of 100-1200 rpm.

3. The method for preparing the multi-level porous boron carbon nitrogen material according to claim 1, characterized in that: In step (3), the off-white solid is transferred to an ark and then placed in a tubular furnace for high-temperature calcination; the ark is made of ceramic, quartz or corundum; the furnace tube in the tubular furnace is made of ceramic, quartz or corundum; the high-temperature calcination temperature is 800-1200°C, and the holding time is 2-8 h; the heating rate of the tubular furnace is 1-10°C / min; and the mixed gas flow rate during calcination is 50-200 mL / min.

4. The multi-level porous boron carbon nitrogen material prepared by the preparation method according to any one of claims 1 to 3.

5. The multi-level porous boron carbon nitride material according to claim 4, characterized in that: The multi-level porous boron carbon nitrogen material is composed of three elements: boron, carbon and nitrogen, and has at least two structures of micropores, mesopores and macropores; wherein the size of the micropores is 0.1-1.8 nm; the size of the mesopores is 10-50 nm; and the size of the macropores is 60-200 nm.

6. Use of the multi-level porous boron carbon nitrogen material according to claim 4 in the activated O2 catalytic oxidation and removal of aromatic sulfides from diesel.