Preparation and application of water-based ink
Through the combination of modified silicone surfactant WG-11 and other formula ingredients, the pH value and surface tension of the ink are adjusted, which solves the problem of ink accumulation at the nozzle of water-based jet printing ink and achieves efficient printing effects and images. quality.
Patent Information
- Application Number
- CN202310161323.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-02-24
AI Technical Summary
The evaporation of water at the nozzle of traditional water-based jet printing ink causes the ink components to precipitate, causing the nozzle to become clogged and affecting the printing effect. Moreover, existing silicone surfactants cannot effectively solve the ink accumulation problem of water-based thermal foaming ink jet, resulting in printing errors. Or the jet is blocked.
Using modified silicone surfactant WG-11, through specific synthesis steps and formulas, the pH value and surface tension of the ink are adjusted, combined with appropriate wetting agents and defoaming agents, to prepare a product that can be used during the printing process. Water-based ink that keeps the ink composition stable and reduces ink accumulation at the nozzle.
The image is clear and complete within 60 minutes of continuous printing, without distortion or missing frames, and there is no ink accumulation at the nozzle, which significantly improves the printing effect and solves the problems of printing errors and nozzle clogging in the traditional ink printing process.
Smart Images

Figure HDA0004199704640000011 
Figure HDA0004199704640000021 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based inks, in particular to water-based inks containing organosilicon surfactants and applications thereof. Background Art
[0002] Traditional water-based inkjet printing ink is a mixture of several components, including volatile solvents, soluble substances and dispersible solids. The inkjet printing ink poured into the ink cartridge is not printed immediately. The water in the ink evaporates quickly at the fixed nozzle without a cap. The water loss will have a great impact on the physical properties and phase behavior of the ink at the nozzle, resulting in poor ignition effect or complete nozzle blockage. This will lead to a deviation in the performance required for inkjet printing, resulting in serious distortion of the printed image, and even nozzle blockage, making it impossible to print.
[0003] If the solvent evaporates significantly at the nozzle, the concentration of certain components in the ink will exceed their solubility, causing these components to precipitate, which means that these stubborn precipitates may clog the nozzle. Similar phenomena can also be seen in pigmented inks. If the concentration of pigment particles increases at the orifice, the particles will agglomerate due to the increased volume content of pigment in the ink. The formation of sticky plugs will hinder the ink jetting, or cause the formation of smaller or slow ink drops. Moreover, the obstruction may completely block the ink jetting or cause the ejected ink drops to go in the wrong direction.
[0004] Thermal inkjet ink must eventually be fixed and dried on the substrate, and there should be some volatile components in it, so sometimes it may happen that the ink cannot be ejected after waiting time. Therefore, inkjet printing ink and ink system should have the ability to restore the ink to its original composition in the nozzle area.
[0005] Ink accumulation on the orifice plate: Some of the ejected ink will inevitably stay on the orifice plate (outside the printhead near the nozzle). The ink accumulated near the nozzle will cause the newly formed ink droplets to lose power, causing printing errors or completely blocking the jet. Therefore, it is necessary to reduce the ink accumulation on the orifice plate.
[0006] If the drop formation process and ink jetting conditions are not optimal, some ink may accumulate on the orifice plate. If the surface tension of the ink is low enough, the ink will spread into a thin layer on the orifice plate, and if evaporated, a solidified layer may form on the orifice plate, hindering ink jetting, depending on the ink jetting mechanism of the printhead and the properties of the wetting film. The wetting of the orifice plate is determined by the surface energy of the constituent materials and the surface tension of the ink. As a rule of thumb, good wettability is achieved when the surface tension of the ink is lower than the surface energy of the orifice plate material. Therefore, the ink configuration can control the surface tension of the ink by selecting the appropriate type and concentration of wetting agents and surfactants, as well as selecting the liquid composition that affects the surface tension and evaporation rate of the liquid medium.
[0007] So far, the selection of ink components seems to be based on some empirical methods, perhaps because other factors need to be considered besides inkjet, and also because the exact chemical composition of most commercial additives (wetting agents, dispersants, etc.) is unknown.
[0008] Water-based thermal jet inks, which reduce surface tension by adding surfactants, have some problems. They often lead to the formation of foam, which prevents normal ink jetting. On the other hand, the problem with the use of surfactants is related to dynamic surface tension, because new interfaces are formed quickly during jetting, and the surfactant may not appear at the newly formed interface, so that the surface tension at this time is higher than the measured value at equilibrium. The time required for the surfactant to diffuse to the interface depends on the structure of the surfactant, which causes the surface tension of the ink drop to continue to change during jetting and flight.
[0009] During the continuous printing process of water-based thermal inkjet, some of the ejected ink will inevitably stay at the orifice plate (outside the nozzle near the nozzle). The accumulated ink near the nozzle will cause the newly formed ink droplets to lose power, causing printing errors or completely blocking the jet. The ink accumulation at the orifice plate can be reduced by adding surfactants. Most of the conventional silicone surfactants on the market cannot solve the problem of ink accumulation during the printing process of water-based thermal inkjet.
[0010] In this patent, a new type of silicone surfactant is added and the water-based ink preparation process is improved, thereby solving the technical problems of printing errors or ink accumulation at the nozzle during the use of water-based ink in the prior art. Summary of the invention
[0011] The purpose of the present invention is to provide a water-based ink containing an organosilicon surfactant and its application.
[0012] A process for preparing a water-based ink containing a modified silicone surfactant comprises the following steps:
[0013] (1) adding a color paste, a moisturizer, an organosilicon surfactant, a defoamer, and deionized water to a reactor in sequence, stirring for 20 minutes at a speed of 500 r / min to obtain a first mixture, wherein the organosilicon surfactant is a product prepared by the present invention;
[0014] (2) adding a pH adjuster to the first mixture obtained in step (1) to adjust the pH value to between 8 and 9, and filtering through a filter membrane with a pore size of 10 μm to obtain an aqueous ink;
[0015] (3) Inject the aqueous ink obtained in step (2) into an ink cartridge and perform a printing test.
[0016] Furthermore, the water-based ink obtained in step (3) was tested and showed that the image was clear and complete without distortion, missing frames or corners, and there was no ink accumulation at the nozzle after continuous printing for 60 minutes.
[0017] Furthermore, the color paste in step (1) contains carbon black, titanium dioxide, lithopone, lead chrome yellow, iron blue and metallic pigments.
[0018] Furthermore, it is characterized in that the moisturizing agent in step (1) is one or more of ethylene glycol, diethylene glycol, propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,2-hexanediol, 1,6-hexanediol or glycerol.
[0019] Furthermore, the defoaming agent in step (1) is Dow Corning DC71.
[0020] Furthermore, in step (1), the pH regulator is triethanolamine, isobutanolamine or urotropine.
[0021] Furthermore, the organosilicon surfactant in step (1) is a modified organosilicon surfactant (numbered WG-11), and the synthesis steps are as follows:
[0022] (1) adding allyl polyether (Formula 1) and 2,3-epoxypropyl methacrylate (GMA, Formula 2) into a reactor and stirring evenly;
[0023]
[0024] Formula 1: Allyl polyether a=0-50, b=0-50, R=H or
[0025]
[0026] Formula 2: 2,3-Epoxypropyl Methacrylate (GMA)
[0027] (2) slowly adding the double-terminal hydrogen-containing silicone oil (Formula 3) to the mixed solution obtained in step (1), while heating it to 80-110° C.;
[0028]
[0029] Formula 3: Low molecular weight double-terminal hydrogen-containing silicone oil m = 0 ~ 10
[0030] (3) After the temperature of the solution obtained in step (2) stabilizes, a catalyst is added dropwise, wherein the catalyst is an isopropanol or tert-butanol solution of chloroplatinic acid, and the reaction is carried out for 7 to 10 hours;
[0031] (4) After the reaction is completed, small molecular oligomers and impurities are removed by vacuum distillation and filtration to obtain a product (Formula 4).
[0032]
[0033] Furthermore, in the step (1) and the step (2), the molar ratio of the double-terminal hydrogen-containing silicone oil, the allyl polyether and the 2,3-epoxypropyl methacrylate is 1:1:1.
[0034] The water-based ink provided by the invention has a simple preparation process and has a significant effect after being used for water-based ink jet printing, thereby solving the technical problems of printing errors or ink accumulation at the nozzle during ink jet printing in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 : Comparison of the printed image after 60 minutes of continuous printing using ink ratio A-3 and the printed image after 60 minutes of continuous printing using ink ratio B-3.
[0036] Figure 2 : Comparison of ink accumulation at the nozzle after printing with different ink ratios: The box marks the position of the nozzle holes of the ink cartridge. Each ink cartridge has two rows of nozzle holes for printing ink; Figure 2 The middle left picture is before inkjet printing. Figure 2 After continuous printing of the middle image with ink ratio A-3 for 60 minutes, Figure 2 The middle right picture shows continuous printing for 60 minutes using ink mix B-3. DETAILED DESCRIPTION
[0037] It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] The performance comparison of water-based inks with WG-11 surfactant or Tego 245 added is shown in Table 1:
[0039] The difference between the A series and the B series is that other ingredients remain unchanged, and WG-11 or Tego245 surfactant is added respectively; the difference between the A-1 / A-2 / A-3 is that different amounts of WG-11 are added respectively; the difference between the B-1 / B-2 / B-3 is that different amounts of Tego245 are added respectively; no surfactant is added to the C series.
[0040] Table 1: List of water-based inks prepared by adding different ratios of surfactants
[0041]
[0042]
[0043] Example 1
[0044] A process for preparing a water-based ink containing an organosilicon surfactant (WG-11) comprises the following steps:
[0045] (1) adding a color paste, a humectant, an organosilicon surfactant (WG-11), a defoamer, and deionized water to a reactor in sequence, stirring for 20 minutes at a speed of 500 r / min to obtain a first mixture, wherein the organosilicon surfactant is a product prepared by the present invention; the color paste contains carbon black, titanium dioxide, lithopone, lead chrome yellow, iron blue, and a metallic pigment; the humectant is ethylene glycol and glycerin; the defoamer is Dow Corning DC71; and the pH regulator is triethanolamine;
[0046] (2) adding a pH adjuster to the first mixture obtained in step (1) to adjust the pH value to between 8 and 9, and filtering through a filter membrane with a pore size of 10 μm to obtain an aqueous ink;
[0047] (3) Inject the aqueous ink obtained in step (2) into an ink cartridge and perform a printing test.
[0048] The water-based ink prepared as above was tested and printed continuously for 60 minutes. The image was clear and complete without distortion, missing frames or corners, and there was no ink accumulation at the nozzle.
[0049] The preparation process of the above-mentioned organosilicon surfactant (WG-11) comprises the following steps:
[0050] (1) adding 1 mol of allyl polyether (a=5, b=5, R=H in Formula 1) and 1 mol of 2,3-epoxypropyl methacrylate into a reactor and stirring evenly;
[0051] (2) slowly adding 1 mol of double-terminal hydrogen-containing silicone oil (in Formula 3, m=2) to the mixed solution obtained in step (1), while heating the solution to 80-90° C.;
[0052] (3) After the temperature of the solution obtained in step (2) stabilizes, a catalyst is added dropwise, wherein the catalyst is an isopropanol solution of chloroplatinic acid containing 0.0005 mol of chloroplatinic acid, and then the reaction is continued for 7 hours;
[0053] (4) After the reaction is completed, small molecular oligomers and impurities are removed by vacuum distillation and filtration to obtain the product (Formula 4, WG-11).
[0054] Example 2
[0055] The formula in Example 1 was adjusted from A-1 to A-2 in Example 2, and the rest was the same as in Example 1 and will not be described in detail.
[0056] Example 3
[0057] The formula in Example 1 was adjusted from A-1 to A-3 in Example 3, and the rest was the same as in Example 1 and will not be described in detail.
[0058] Example 4
[0059] The pH regulator in Example 1 was adjusted to hexamethylenetetramine, and the rest was the same as in Example 1 and will not be described in detail.
[0060] Comparative Example 1
[0061] The formula in Example 1 was adjusted from A-1 to B-1 in Comparative Example 1, and the rest was the same as in Example 1 and will not be described in detail.
[0062] Comparative Example 2
[0063] The formula in Example 1 was adjusted from A-1 to B-2 in Comparative Example 2, and the rest was the same as in Example 1 and will not be described in detail.
[0064] Comparative Example 3
[0065] The formula in Example 1 was adjusted from A-1 to B-3 in Comparative Example 3, and the rest was the same as in Example 1 and will not be described in detail.
[0066] Comparative Example 4
[0067] The formula in Example 1 was adjusted from A-1 to C in Comparative Example 4, and the rest was the same as in Example 1 and will not be described in detail.
[0068] The dynamic surface tension of the water-based ink prepared in the above examples and comparative examples is shown in Table 2:
[0069] Table 2: Dynamic surface tension of water-based inks prepared in the above examples and comparative examples
[0070]
[0071]
[0072] The data in the table above show that the surface tension decreases with time. When WG-11 is added at 0.3%, the surface tension of the ink is 48.32 mN / m at 15 ms, which meets the requirement of surface tension less than 50 mN / m.
[0073] There is a gas-liquid interface at the nozzle of water-based inkjet, and the force from the surface of the liquid interface molecules to the inside of the liquid is called surface tension. Adding surfactants to the ink will affect the surface tension of the ink. After the ink droplets are ejected, when a new interface is formed, it takes time for the surfactant to migrate to the new interface. A thermal inkjet nozzle ejects about 10,000 to 30,000 ink droplets per second, that is, the time interval before and after the ink is printed is less than 100 microseconds, that is, the time for the surfactant to migrate from the inside to the ink surface at the nozzle is less than 100us.
[0074] The time required for a surfactant to diffuse to the interface depends on the chemical structure of the surfactant, so surfactants with different chemical structures diffuse to the interface at different rates.
[0075] It can be observed from the data in Table 2 that the performance of adding WG-11 is better than that of Tego245.
[0076] After 60 minutes of continuous printing, the printed pattern is relatively clear. Figure 1 :
[0077] It can be observed that:
[0078] 1. Using the A-3 ink, after 60 minutes of continuous printing, the image is clear and complete without distortion or missing frames or corners.
[0079] 2. After 60 minutes of continuous printing with B-3 ink, the image is blurred and distorted, with obvious missing frames and corners. This is because the accumulated ink overflowed from the nozzle, blocking the nozzle hole and hindering printing.
[0080] Comparison of ink accumulation at the nozzle after printing with different ink ratios:
[0081] Using ink ratio A-3 or B-3, after continuous printing for 60 minutes, the ink accumulation at the nozzle is as follows Figure 2 :
[0082] Nozzle description: The boxes mark the positions of the ink cartridge nozzle holes. Each ink cartridge has two rows of holes for printing ink. The three pictures above show the left picture before inkjet printing.
[0083] It can be observed that: using ink ratio A-3 (the three figures above, the middle figure), after 60 minutes of continuous printing, there is no obvious accumulation of ink at the nozzle.
[0084] Using ink ratio B-3 (three figures above, right figure), after 60 minutes of continuous printing, there is obvious accumulation of ink at the nozzle.
Claims
1. A method for preparing a water-based ink containing a modified silicone surfactant, The following steps are involved: (1) Adding a color paste, a moisturizing agent, a modified silicone surfactant, a defoaming agent, and deionized water to a reactor in sequence, and stirring evenly to obtain a first mixture; (2) adding a pH adjuster to the first mixture obtained in step (1) to adjust the pH value to between 8 and 9, and filtering through a filter membrane with a pore size of 10 μm to obtain a water-based ink; (3) injecting the aqueous ink obtained in step (2) into an ink cartridge and performing a printing test; in, In step (2), the pH regulator is triethanolamine, isobutanolamine or hexamethylenetetramine; The synthesis steps of the modified silicone surfactant described in step (1) are as follows: S1: Take allyl polyether as shown in formula 1 and 2,3-epoxypropyl methacrylate GMA as shown in formula 2, add them into a reactor, and stir evenly; S2: slowly add the double-terminal hydrogen-containing silicone oil, as shown in Formula 3, to the mixed solution obtained in S1, while heating it to 80-90°C; S3: After the temperature of the solution obtained in S2 stabilizes, a catalyst is added dropwise, wherein the catalyst is an isopropanol solution of chloroplatinic acid or a tert-butanol solution of chloroplatinic acid, and the reaction time is 7 hours; S4: After the reaction is completed, small molecular oligomers and impurities are removed by vacuum distillation and filtration to obtain a product, a modified silicone surfactant as shown in Formula 4; The molar ratio of the double-terminal hydrogen-containing silicone oil in S2 to the allyl polyether and 2,3-epoxypropyl methacrylate in S1 is 1:1:
1.
2. The preparation method according to claim 1, It is characterized in that The color paste in step (1) contains carbon black, titanium dioxide, lithopone, lead chrome yellow, iron blue and metallic pigments.
3. The preparation method according to claim 1, It is characterized in that In step (1), the moisturizing agent is one or more of ethylene glycol, diethylene glycol, propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,2-hexanediol, 1,6-hexanediol or glycerol.