A Cu-containing nanostructured carbon monoxide adsorption + Adsorbent and preparation method and application thereof

By calculating Cu+ precursor at high temperature on a carbon support, avoiding oxidation or reduction of Cu+ ions, Cu+ adsorbents containing high CO adsorption capacity are prepared, and the problem of Cu+ ion reaction in the prior art forms other crystal phases is solved, and the adsorbent is realized Highly efficient CO adsorption and good regeneration performance.

CN116712972BActive Publication Date: 2024-12-06ZHEJIANG UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310356627.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-12-06
Estimated Expiration
2043-03-31

AI Technical Summary

Technical Problem

During the preparation of existing carbon-carrying copper adsorbents, Cu+ ions are easily oxidized or reduced, forming other copper-containing crystal phases, resulting in low CO adsorption.

Method used

Using carbon-containing materials with suitable surface groups, texture and chemical composition as support, the Cu+ precursor and carbon support are treated by high-temperature calcination to avoid Cu+ ions forming crystal phases of other Cu0 or Cu2+ species, and a high CO adsorption capacity is prepared. Cu+ adsorbent.

Benefits of technology

The high dispersion of Cu+ species on the surface of carbon support is achieved, the CO adsorption amount is increased, and the prepared adsorbent can be directly used in fixed bed reactors without further reduction or activation pretreatment, showing good CO adsorption and regeneration properties. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004163520950000011
    Figure HDA0004163520950000011
  • Figure HDA0004163520950000012
    Figure HDA0004163520950000012
  • Figure HDA0004163520950000021
    Figure HDA0004163520950000021
Patent Text Reader

Abstract

The invention discloses a Cu-containing + Adsorbent and its preparation method and application. + The adsorbent is prepared by + The precursor and the carbon carrier are mixed in liquid phase and dispersed uniformly. The obtained slurry is filtered and dried to obtain an adsorbent precursor. The adsorbent precursor is obtained by high-temperature calcination in an inert atmosphere. + The adsorbent does not contain Cu 0 Cu 2+ The specific surface area of ​​the carbon carrier is not less than 800m 2 g ‑1 , wherein the external specific surface area accounts for no less than 45%; the surface carboxyl amount of the carbon carrier is no less than 0.0012 mmol / m 2 The present invention realizes Cu + The high dispersion of species on the surface of the carbon support avoids the formation of other Cu-containing 0 Cu 2+ The crystal phase of the species is thus solved in the preparation process of the existing carbon carrier copper adsorbent, which is easy to make Cu + The ions undergo oxidation or reduction reactions to form other copper-containing crystalline phases, resulting in low CO adsorption capacity and other problems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a Cu-containing + Adsorbent and preparation method and application thereof. Background Art

[0002] CO molecules are not only the main component of synthesis gas, but also an important raw material for synthesizing many organic chemical products. At present, gasification through water gas, coal or coke is the main method for industrial production of CO, but its purity is not high. On the other hand, CO molecules in the gas can easily cause poisoning and deactivation of metal catalysts. Based on the above reasons, the separation and purification of CO molecules has very important industrial application value. At present, the main CO separation processes include cryogenic separation, solution absorption and adsorption separation. For industrial application processes, cryogenic separation, solution absorption and other methods have high requirements for process equipment, high energy consumption in the process, and complex regeneration conditions. In comparison, the adsorption separation process is simple and the regeneration conditions are mild, but the development of efficient adsorbents is a key issue.

[0003] According to the difference in the force, adsorption can be divided into physical adsorption, chemical adsorption and complex adsorption. Complex adsorption is the separation of gases through the π-complex interaction between the active components on the adsorbent and the adsorbate. Combining the adsorption separation process with the reversible characteristics of π-complexation, the complex adsorbent has the advantages of large adsorption capacity, high selectivity, mild reaction conditions and good regeneration. Transition metal Cu + The ions can form metal carbonyl compounds with CO molecules through π complexation, thereby achieving the purpose of selectively adsorbing CO molecules in the mixed gas. + Ions are dispersed on various carriers (e.g. molecular sieves, MOFs, activated carbon, etc.) to prepare copper-loaded adsorbents suitable for CO molecule adsorption. Compared with other carriers such as molecular sieves, activated carbon materials have the advantages of low price, high specific surface area and high chemical corrosion resistance, so they are excellent carriers for preparing copper-loaded adsorbents. However, due to the properties of carbon materials and their surface groups, it is easy to make Cu ions in the loading process. + The ions undergo oxidation or reduction reactions to form other copper species, thereby reducing the CO adsorption performance of the copper-loaded adsorbent.

[0004] Therefore, the present invention mainly relates to a Cu-containing + Preparation method of adsorbent. By selecting a carbon-containing material with suitable surface groups, texture and chemical composition as a carrier, a mixture of cuprous chloride precursor and carbon-containing material is subjected to high-temperature calcination treatment at a suitable temperature and atmosphere to achieve Cu + The high dispersion of species on the surface of the carbon support avoids the formation of other Cu-containing 0 or Cu 2+On this basis, the copper-loaded adsorbent prepared by the method of the present invention can be directly loaded into a fixed bed stainless steel reactor without further reduction or activation pretreatment, and adsorbs CO molecules from the mixed gas by selective adsorption. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a Cu-containing material with high CO adsorption capacity. + Adsorbent and preparation method and application thereof, using carbonaceous materials with suitable surface groups, textures and chemical compositions as carriers to achieve Cu + The high dispersion of species on the surface of the carbon support avoids the formation of other Cu-containing 0 Cu 2+ The crystal phase of the species is thus solved in the preparation process of the existing carbon carrier copper adsorbent, which is easy to make Cu + The ions undergo oxidation or reduction reactions to form other copper-containing crystalline phases, which leads to problems such as low CO adsorption.

[0006] The technical solution adopted to solve the above technical problems is described below.

[0007] In a first aspect, the present invention provides a Cu-containing + The adsorbent is prepared by + The precursor and the carbon carrier are mixed in liquid phase and dispersed uniformly. The obtained slurry is filtered and dried to obtain an adsorbent precursor. The adsorbent precursor is obtained by high-temperature calcination in an inert atmosphere. + The adsorbent does not contain Cu 0 Cu 2+ The specific surface area of ​​the carbon carrier is not less than 800m 2 g -1 , wherein the external specific surface area accounts for no less than 45%; the surface carboxyl amount of the carbon carrier is no less than 0.0012 mmol / m 2 The surface of the carbon carrier mainly contains C, O, N and Si elements, with the total content of C, O, N and Si elements being 100%, wherein the percentage of C element is 75-85at.%, the percentage of Si element is 1-5at.%, the percentage of N element is 1-5at.%, and the percentage of O element is 10-15at.%.

[0008] Preferably, the external specific surface area of ​​the carbon carrier accounts for 45-50%, and the amount of carboxyl groups on the surface of the carbon carrier is 0.0012-0.0016 mmol / m 2 .

[0009] The carbon carrier used in the present invention can use commercial products that meet the above requirements, or commercial products that do not fully meet the requirements can be pretreated accordingly to obtain carbon carriers that meet the requirements. In a specific embodiment of the present invention, the activated carbon produced by Pingdingshan Green Forest Activated Carbon Co., Ltd. is pretreated with a nitric acid aqueous solution with a concentration of 25-30%. The pretreatment conditions are: pretreatment at 80-90°C for 4-5 hours, then washing until the pH value of the filtrate is close to neutral, and then drying and grinding to obtain the carbon carrier. Preferably, the concentration of the nitric acid aqueous solution is 28%. Preferably, the drying conditions are: drying at 100-120°C in an air atmosphere for 4-6 hours. Preferably, the carbon carrier is ground to a mesh size of 80 or more.

[0010] Preferably, the Cu-containing + The precursor is CuCl.

[0011] Preferably, the carbon support is + The mass ratio of the precursors is 2:1.

[0012] Preferably, the Cu-containing + After the precursor and the carbon carrier are mixed in liquid phase, the mixture is stirred in a magnetic stirrer at a speed of 150-200 r / min for 10-20 minutes, and then placed in an ultrasonic cleaner for ultrasonic oscillation at a power of 90-110 W for 30-40 minutes to obtain a slurry.

[0013] Preferably, the high temperature calcination temperature is 250-350°C.

[0014] In a second aspect, the present invention provides a Cu-containing + The preparation method of the adsorbent comprises the following steps:

[0015] (a) obtaining a powdered carbon carrier, wherein the carbon carrier has a specific surface area of ​​not less than 800 m 2 g -1 , wherein the external specific surface area accounts for no less than 45%; the amount of carboxyl groups on the surface of the carbon carrier is no less than 0.0012 mmol / m 2 The surface of the carbon carrier mainly contains C, O, N and Si elements, wherein the C element percentage is 75-85at.%, the Si element percentage is 1-5at.%, the N element percentage is 1-5at.%, and the O element percentage is 10-15at.%;

[0016] (b) The obtained powdered carbon support is mixed with Cu +The precursor and the solvent are mixed to obtain a mixture, the mixture is stirred in a magnetic stirrer at a speed of 150-200 r / min for 10-20 minutes, and then placed in an ultrasonic cleaner for ultrasonic oscillation at a power of 90-110 W for 30-40 minutes to obtain a slurry, and the obtained slurry is filtered and dried to obtain an adsorbent precursor;

[0017] (c) calcining the adsorbent precursor obtained in step (b) at 250-350° C. in an inert atmosphere to obtain the Cu-containing + Adsorbent.

[0018] Preferably, the external specific surface area of ​​the carbon carrier accounts for 45-50%, and the amount of carboxyl groups on the surface of the carbon carrier is 0.0012-0.0016 mmol / m 2 .

[0019] Preferably, in step (b), the Cu-containing + The precursor is CuCl, the solvent is n-hexane, the powdered carbon carrier and the Cu + The mass ratio of the precursors is 2: 1. The amount of the solvent used is 10-20 mL / g based on the mass of the powdered carbon carrier.

[0020] Preferably, in step (b), the drying conditions are: vacuum drying at 100-120° C. for 4-6 hours.

[0021] Preferably, in step (c), the inert atmosphere is selected from N2, Ar or He, more preferably N2, the purity of which is not less than 99.999%.

[0022] Preferably, in step (c), the inert gas flow rate is 80-105 mL / min, and the heating rate is 3-6° C. / min.

[0023] Preferably, in step (c), the calcination temperature is 350°C and the calcination time is 4 hours. This calcination condition is conducive to protecting Cu + It is neither oxidized nor reduced to metallic copper, and is beneficial to Cu + Highly dispersed on the carrier surface.

[0024] In a third aspect, the present invention provides the Cu-containing + Application of the adsorbent in the CO adsorption process, the Cu-containing + The adsorbent does not require reduction or activation pretreatment and can be directly loaded into a fixed bed reactor for adsorption application. + The adsorbent exhibited good CO adsorption and regeneration performance.

[0025] Preferably, the application is carried out at room temperature.

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] (1) The preparation method reported in the present invention is conducive to obtaining Cu-containing + The adsorbent of the present invention solves the problem that the existing carbon carrier copper adsorbent is easy to make Cu + The problem of ions undergoing oxidation or reduction reactions to form other copper-containing crystalline phases, and the prepared Cu-containing + The adsorbent does not require reduction or activation pretreatment and can be directly loaded into a fixed bed reactor to participate in the adsorption reaction.

[0028] (2) The Cu-containing + The adsorbent has a large CO adsorption capacity and can be regenerated and recycled by increasing the temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The Cu-containing + XRD patterns of the adsorbents.

[0030] Figure 2 The Cu-containing + XRD patterns of the adsorbents.

[0031] Figure 3 The Cu-containing + XRD patterns of the adsorbents.

[0032] Figure 4 The Cu-containing + XRD patterns of the adsorbents. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described below with specific embodiments, but the protection scope of the present invention is not limited by the following embodiments.

[0034] Example 1

[0035] Measure 64.62mL of 65-68% HNO3 solution and dissolve it in 85.38mL of deionized water at room temperature to obtain 150mL of 28% nitric acid aqueous solution. Weigh 20g of AC-1 activated carbon carrier (manufacturer: Pingdingshan Lvlin Activated Carbon Co., Ltd.) and add it to a three-necked flask, add the prepared nitric acid aqueous solution to the flask and put it into a rotor, stir and heat it in an 80℃ oil bath for 4h, lift the flask after the end, filter and wash it after cooling to room temperature until the filtrate pH is ≈ 7, put it in an oven and dry it at 120℃ for 6h, grind the dried carrier into a powder of more than 80 mesh in an agate mortar, and store it in a dryer for use. The specific surface area of ​​the AC-1 carbon-containing carrier powder after the above treatment is 891.31m2 ·g -1 The external specific surface area accounts for 46% and the surface carboxyl content is 0.00157mmol / m 2 The C element content on the surface of the material is 80.04at.%, the O element content is 14.53at.%, the N element content is 1.67at.%, and the Si element content is 3.76at.%.

[0036] 2g of CuCl powder and 4g of AC-1 carbon-containing carrier powder treated as above were weighed in a beaker at a mass ratio of 0.5:1, and 40mL of n-hexane was added to the beaker to obtain a mixed solution A. After the mixed solution A was stirred with a magnetic stirrer (175r / min) for 10 minutes, it was placed in an ultrasonic cleaner (ultrasonic power 100W) for ultrasonic oscillation for 30 minutes. After filtering the slurry, the resulting mixture was dried in a vacuum oven at 120°C for 4 hours to obtain a copper-loaded adsorbent precursor. The adsorbent precursor was placed in a tubular furnace, and in a 99.999% high-purity nitrogen atmosphere, the temperature was raised to 350°C at a gas flow rate of 100mL / min and a heating rate of 5°C / min, and then calcined for 4 hours to obtain AC-1-0.5 copper-loaded adsorbent. Attached Figure 1 The XRD spectrum of the AC-1-0.5 copper-carrying adsorbent prepared in Example 1 shows that only CuCl species exist in the adsorbent, indicating that the carbon-containing carrier and preparation method described in Example 1 can form Cu on the surface of the AC-1 carrier. + Species, no other Cu-containing 0 or Cu 2+ Crystalline phase of the species.

[0037] Comparative Example 1

[0038] Measure 64.62mL of 65-68% HNO3 solution and dissolve it in 85.38mL of deionized water at room temperature to obtain 150mL of 28% nitric acid aqueous solution. Weigh 20g of AC-3 capacitor carbon carrier (manufacturer: Jiangsu Xinghong Carbon Technology Co., Ltd., ash content ≤0.15%) and add it to a three-necked flask. Add the above-prepared nitric acid aqueous solution to the three-necked flask and put it into the rotor. Stir and heat it in an 80℃ oil bath for 4h. After the end, lift the flask, cool it to room temperature, filter and wash it until the filtrate pH is ≈7, put it in an oven and dry it at 120℃ for 6h. Grind the dried carrier into a powder of more than 80 mesh in an agate mortar and store it in a dryer for standby use. The specific surface area of ​​the AC-3 capacitor carbon carrier powder after the above treatment is 1464.53m 2 ·g -1 The external specific surface area accounts for 31.5%, and the surface has 0.001mmol / m 2 carboxyl.

[0039] Weigh CuCl powder and AC-3 capacitive carbon carrier powder treated as above in a mass ratio of 0.8:1 and place them in a beaker, and add 40 mL of n-hexane to the beaker to obtain a mixed solution A. Stir the mixed solution A with a magnetic stirrer (175 r / min) for 10 min, and then place it in an ultrasonic cleaner (ultrasonic power 100 W) for ultrasonic oscillation for 30 min. After filtering the slurry, the resulting mixture was dried in a vacuum oven at 120 ° C for 4 h to obtain a copper-loaded adsorbent precursor. The adsorbent precursor was placed in a tubular furnace, and calcined at 350 ° C for 4 h in a 99.999% high-purity nitrogen atmosphere (100 mL / min, heating rate 5 ° C / min) to obtain the AC-3-0.8 adsorbent. Attached Figure 2 This is the XRD spectrum of AC-3-0.8 adsorbent. This figure shows that in addition to the diffraction peaks attributable to the CuCl crystal phase, the adsorbent also has diffraction peaks attributable to Cu 0 diffraction peaks.

[0040] Comparison of Example 1 with Example 1 shows that carbonaceous material carriers with different chemical compositions, specific surface areas and surface groups have an important influence on the type of Cu species loaded. The use of AC-3 capacitor carbon carrier with low ash content can transfer part of the Cu + Reduction to form Cu 0 crystalline phase, but reduced the Cu + Species content.

[0041] Comparative Example 2

[0042] Measure 64.62mL of 65-68% HNO3 solution and dissolve it in 85.38mL of deionized water at room temperature to obtain 150mL of 28% nitric acid aqueous solution. Weigh 20g of AC-3 capacitor carbon carrier (manufacturer: Jiangsu Xinghong Carbon Technology Co., Ltd., ash content ≤0.15%) and add it to a three-necked flask. Add the above-prepared nitric acid aqueous solution to the three-necked flask and put it into the rotor. Stir and heat it in an 80℃ oil bath for 4h. After the end, lift the flask, cool it to room temperature, filter and wash it until the filtrate pH is ≈7, put it in an oven and dry it at 120℃ for 6h. Grind the dried carrier into a powder of more than 80 mesh in an agate mortar and store it in a dryer for standby use. The specific surface area of ​​the AC-3 capacitor carbon carrier powder after the above treatment is 1464.53m 2 ·g -1 The external specific surface area accounts for 31.5%, and the surface has 0.001mmol / m 2 carboxyl.

[0043] Weigh CuCl powder and AC-3 capacitive carbon carrier powder treated as above in a mass ratio of 1.1:1 and place them in a beaker, and add 40 mL of n-hexane to the beaker to obtain a mixed solution A. Stir the mixed solution A with a magnetic stirrer (175 r / min) for 10 min, and then place it in an ultrasonic cleaner (ultrasonic power 100 W) for ultrasonic oscillation for 30 min. After filtering the slurry, the resulting mixture was dried in a vacuum oven at 120 ° C for 4 h to obtain a copper-loaded adsorbent precursor. The adsorbent precursor was placed in a tubular furnace and calcined at 350 ° C for 4 h in a 99.999% high-purity nitrogen atmosphere (100 mL / min, heating rate 5 ° C / min) to obtain the AC-3-1.1 adsorbent. Attached Figure 3 This is the XRD spectrum of AC-3-1.1 adsorbent. This figure shows that the adsorbent not only has diffraction peaks attributable to CuCl, but also has diffraction peaks attributable to Cu 0 diffraction peaks.

[0044] The above comparative examples show that according to the ratio of the specific surface areas of AC-3 to AC-1 (~1.6), increasing the amount of CuCl (0.8 g) in proportion does not form only CuCl crystal phase on the AC-3 carbon support, but forms Cu 0 Further increasing the CuCl precursor loading, CuCl and Cu 0 By comparing Example 1 with Comparative Examples 1 and 2, it is shown that the use of AC-1 carbon-containing carrier is effective in maintaining and dispersing Cu on the surface of the carbon-containing carrier. + Species plays an important role.

[0045] Comparative Example 3

[0046] Measure 64.62mL of 65-68% HNO3 solution and dissolve it in 85.38mL of deionized water at room temperature to obtain 150mL of 28% nitric acid aqueous solution. Weigh 20g of AC-1 activated carbon carrier (manufacturer: Pingdingshan Lvlin Activated Carbon Co., Ltd.) and add it to a three-necked flask, add the prepared nitric acid aqueous solution to the flask and put it into a rotor, stir and heat it in an 80℃ oil bath for 4h, lift the flask after the end, filter and wash it after cooling to room temperature until the filtrate pH is ≈ 7, put it in an oven and dry it at 120℃ for 6h, grind the dried carrier into a powder of more than 80 mesh in an agate mortar, and store it in a dryer for use. The specific surface area of ​​the AC-1 carbon-containing carrier powder after the above treatment is 891.31m 2 ·g -1 The external specific surface area accounts for 46% and the surface carboxyl content is 0.00157mmol / m 2The C element content on the surface of the material is 80.04at.%, the O element content is 14.53at.%, the N element content is 1.67at.%, and the Si element content is 3.76at.%.

[0047] Weigh CuCl powder and ground AC-1 carbon-containing carrier in a beaker at a mass ratio of 0.5:1, stir with a glass rod for 2 minutes to mix them evenly, and obtain a copper-loaded adsorbent precursor. Place the adsorbent precursor in a tube furnace, and heat it to 350°C in a 99.999% high-purity nitrogen atmosphere at a gas flow rate of 100mL / min and a heating rate of 5°C / min for 4 hours to obtain a copper-loaded adsorbent. Figure 4 The XRD spectrum of the adsorbent prepared by the method described in Comparative Example 3 shows that the adsorbent contains CuCl crystal phase and Cu 0 and CuCl2·3Cu(OH)2 crystal phases, which indicates that part of the CuCl precursor underwent oxidation and reduction reactions during the preparation process described in Comparative Example 3. By comparing Example 1 with Comparative Example 3, it is shown that even on the basis of using the AC-1 carbon-containing support, only by using a suitable preparation method can Cu be maintained and dispersed on the surface of the AC-1 carbon-containing support. + species, avoid the presence of other Cu 0 or Cu 2+ Crystalline phase of the species.

[0048] Comparative Example 4

[0049] The commercial 5A molecular sieve (Southwest Chemical Research and Design Institute Co., Ltd., with a specific surface area of ​​514.13 m 2 ·g -1 ) After drying at 100°C for 4 hours, grind into powder above 80 mesh, then weigh CuCl powder and ground 5A molecular sieve powder in a mass ratio of 0.5:1 and place them in a beaker, and add 40mL of n-hexane to the beaker to obtain a mixed solution A. After stirring the mixed solution A with a magnetic stirrer (175r / min) for 10 minutes, place it in an ultrasonic cleaner (ultrasonic power 100W) for ultrasonic oscillation for 30 minutes. After filtering the slurry, the resulting mixture is dried in a vacuum oven at 120°C for 4 hours to obtain a copper-loaded molecular sieve adsorbent precursor. The adsorbent precursor is placed in a tube furnace and calcined at 350°C for 4 hours in a 99.999% high-purity nitrogen atmosphere (100mL / min, heating rate 5°C / min) to obtain a 0.5Cu / 5A copper-loaded molecular sieve adsorbent.

[0050] Example 2

[0051] A fixed bed reactor was used to conduct a CO molecule adsorption performance evaluation test experiment on the adsorbents prepared by Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 4. The samples were loaded into a stainless steel reaction tube in the order of gauze-quartz wool-adsorbent-quartz wool-gauze. The reaction tube was 25 cm long, 2 cm in inner diameter, and 5 g in adsorbent loading. The adsorption temperature was room temperature, the pressure was 1 MPa, CO / (Ar+CO) in the raw gas was 10%, and the adsorption amount was calculated by determining the CO adsorption penetration time through continuous gas intake and chromatographic signal intensity.

[0052] CO dynamic adsorption amount = adsorption breakthrough time × actual CO gas flow rate / adsorbent mass

[0053] The results of the adsorption test show that under the conditions of room temperature, 1MPa, and CO / (Ar+CO)=10%, the CO adsorption capacity of AC-1-0.5 adsorbent is 46.87mL / g, the CO adsorption capacity of AC-3-0.8 adsorbent is 28.25mL / g, the CO adsorption capacity of AC-3-1.1 adsorbent is 38.09mL / g, and the CO adsorption capacity of 0.5Cu / 5A adsorbent is 33.60mL / g. The above experimental results show that the Cu-containing adsorbent prepared with AC-1 carbonaceous material as the carrier + The CO adsorption capacity of the adsorbent (AC-1-0.5) is higher than that of the Cu-containing adsorbent prepared with 5A molecular sieve and AC-3 capacitor carbon as carriers. + Adsorbents (AC-3-0.8, AC-3-1.1 and 0.5Cu / 5A).

[0054] Furthermore, the temperature was raised to 600°C under 99.999% high-purity nitrogen atmosphere at a gas flow rate of 100 mL / min and a heating rate of 5°C / min, and the AC-1-0.5 adsorbent after the adsorption reaction was desorbed under high temperature conditions for 1 hour, and the adsorption reaction of the desorbed AC-1-0.5 adsorbent was evaluated again. The above operation was repeated twice, and the adsorption amounts were 43.14 mL / g and 42.44 mL / g, respectively. This proves that after the temperature desorption treatment, the CO adsorption amount of the AC-1-0.5 adsorbent did not change significantly, and the adsorbent had good regeneration performance.

[0055] The various performance parameters of the carbon carrier in the present invention are measured by the following method:

[0056] 1. Use Boehm titration method to detect the surface carboxyl content of carbon materials:

[0057] First, prepare 0.05mol / L NaOH, NaHCO3 and HCl solutions. Then weigh 0.5g phenolphthalein, dissolve it in a small amount of 95% ethanol, and then dilute it to 100mL to prepare phenolphthalein indicator solution. Use an electronic balance to accurately weigh 1g of carbon material sample, put it in a small beaker with a volume of 100mL, add 25mL of NaHCO3 solution with a concentration of 0.05mol / L, stir for 24h, and then filter and collect the filtrate. Add 50mL of hydrochloric acid solution (0.05mol / L) to the filtrate, use phenolphthalein as the end point indicator, and titrate the excess hydrochloric acid in the filtrate with 0.05mol / L NaOH solution to the end point. The alkali consumption is calculated using the following formula:

[0058] n 碱 =(V×C NaOH +25×C0-50×C HCl ) / m C

[0059] n in the formula 碱 is the amount of alkali consumed (mmol / g); V is the volume of NaOH standard solution consumed (mL); C NaOH is the concentration of NaOH standard solution; 25 is the volume of alkali solution used (mL); C0 is the concentration of alkali solution used, 50 is the volume of hydrochloric acid (mL), C HCl is the concentration of the hydrochloric acid solution used, m C is the mass of carbon material (g).

[0060] The alkali consumption is calculated according to the above formula to obtain the amount of carboxyl groups on the surface of the carbon material:

[0061] n(RCOOH)=n(NaHCO3)

[0062] On this basis, the specific surface area of ​​the carbon material obtained by low-temperature N2 adsorption characterization is further normalized to obtain the carboxyl values ​​described in the embodiments of the present invention and the comparative examples.

[0063] 2. The textural properties of the carbon material of the present invention were analyzed using a low-temperature N2 physical adsorption-desorption instrument (Micromeritics 3Flex):

[0064] First, take ~0.1g sample and pre-treat and degas for 5h at 200℃ to remove impurity gas and water on the sample surface. The treated sample is placed in liquid nitrogen for low-temperature N2 physical adsorption-desorption experiment. The specific surface area of ​​the sample in the present invention is calculated by BET equation, and the external specific surface area is calculated by t-Plot method.

[0065] 3. The elemental composition of the surface of the carbon material of the present invention is analyzed by X-ray photoelectron spectrometer (ThermoKalpha) using an Al target X-ray source.

Claims

1. A Cu-containing catalyst for CO adsorption + The preparation method of the adsorbent is characterized by: The preparation method comprises the following steps: (a) obtaining a powdered carbon carrier, wherein the carbon carrier has a specific surface area of ​​not less than 800 m 2 g -1 , wherein the external specific surface area accounts for no less than 45%; the amount of carboxyl groups on the surface of the carbon carrier is no less than 0.0012 mmol / m 2 The surface of the carbon carrier mainly contains C, O, N and Si elements, with the total content of C, O, N and Si elements being 100%, wherein the percentage of C element is 75-85 at.%, the percentage of Si element is 1-5 at.%, the percentage of N element is 1-5 at.%, and the percentage of O element is 10-15 at.%; (b) The obtained powdered carbon support is mixed with Cu + The precursor and the solvent are mixed to obtain a mixture, the mixture is stirred in a magnetic stirrer at a speed of 150-200 r / min for 10-20 minutes, and then placed in an ultrasonic cleaner for ultrasonic oscillation at a power of 90-110 W for 30-40 minutes to obtain a slurry, and the obtained slurry is filtered and dried to obtain an adsorbent precursor; (c) calcining the adsorbent precursor obtained in step (b) at 250-350° C. in an inert atmosphere to obtain the Cu-containing + The adsorbent contains Cu + The adsorbent does not contain Cu 0 Cu 2+ Crystalline phase of the species.

2. The preparation method according to claim 1, characterized in that: In step (b), the Cu-containing + The precursor is CuCl, the solvent is n-hexane, the powdered carbon carrier and the Cu + The mass ratio of the precursors is 2:

1.

3. The preparation method according to claim 1, characterized in that: The external specific surface area of ​​the carbon carrier accounts for 45-50%, and the amount of carboxyl groups on the surface of the carbon carrier is 0.0012-0.0016 mmol / m 2 .

4. The preparation method according to claim 1, characterized in that: In step (b), the drying conditions are: vacuum drying at 100-120° C. for 4-6 hours.

5. The preparation method according to claim 1, characterized in that: In step (c), the inert gas flow rate is 80-105 mL / min, and the heating rate is 3-6° C. / min.

6. The preparation method according to claim 1, characterized in that: In step (c), the calcination temperature is 350° C. and the calcination time is 4 h.

7. The Cu-containing + Application of the adsorbent in the CO adsorption process, the Cu-containing + The adsorbent does not require reduction or activation pretreatment and can be directly loaded into a fixed bed reactor for adsorption applications.