A method for preparing spinel carbon material with low thermal expansion coefficient

By pretreating spinel particles to form a thin film, combined with scale graphite and phenolic resin, the thermal expansion rate of spinel carbon material is reduced, and the problem of fracture of spinel carbon material and aluminum carbon material composite at high temperature is solved. , improves thermal shock resistance and stability.

CN116715530BActive Publication Date: 2024-11-22SINOSTEEL LUOYANG INSTITUTE OF REFRACTORIES RESEARCH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310645274.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-11-22
Estimated Expiration
2043-06-02

AI Technical Summary

Technical Problem

The high thermal expansion rate of spinel carbon material leads to fracture of the joint site with the aluminum-carbon material composite at high temperatures, affecting production efficiency, and the difference in thermal expansion rate leads to poor thermal shock resistance.

Method used

By pretreating spinel particles, wax, silicon sol and PVA films are formed, combined with scale graphite and phenolic resin, dried and heat-treated to form spinel carbon material with low thermal expansion, and the thermal expansion is counteracted using surface holes.

Benefits of technology

It significantly reduces the thermal expansion rate of spinel carbon material, improves its thermal shock resistance and stability, and reduces the fracture situation with the aluminum-carbon material composite.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of refractory materials, and relates to a method for preparing a spinel carbon material with low thermal expansion rate. The method for preparing a spinel carbon material with low thermal expansion rate involves pre-treating spinel particles, that is, mixing spinel particles with one of wax, silica sol, and PVA, and forming a thin film on the surface of spinel particles; the amount of wax, silica sol, and PVA added is 1-5% of the spinel particles; the mixed spinel raw material is dried; according to the mass percentage, the above-mentioned pre-treated spinel particles, flake graphite, spinel fine powder, and phenolic resin are mixed in a mixer to form a spinel carbon raw material, dried and cold isostatically pressed, and heat treated at 950°C for 5h to prepare a spinel carbon material with low thermal expansion rate. The present invention reduces the thermal expansion rate of spinel carbon material products; and has good thermal shock resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a method for preparing a spinel carbon material with a low thermal expansion coefficient. Background Art

[0002] Spinel carbon material has high melting point and high strength, and has excellent resistance to erosion and corrosion of molten steel. It can be used in parts with harsh service environments such as integral stopper rod heads and submerged nozzle bowls, and can be used in combination with aluminum-carbon materials. However, the thermal expansion rate of spinel material is too high. The thermal expansion rate of theoretical stoichiometric spinel material at 1300℃ can reach 8.5%. Even if the spinel carbon material contains a certain amount of graphite, which reduces the thermal expansion rate, its thermal expansion rate at 1300℃ is still more than 7%, while the thermal expansion rate of aluminum-carbon material at 1300℃ is about 4%. Due to the large difference in thermal expansion rate between spinel carbon material and aluminum-carbon material, in addition, the greater the thermal expansion rate of refractory materials, the worse their thermal shock resistance; therefore, during use, the integral stopper rod and submerged nozzle composited with spinel carbon material and aluminum-carbon material often break at the joint, causing production interruption and affecting production efficiency. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a spinel carbon material with low thermal expansion coefficient, so as to improve the stability of the product during use.

[0004] The present invention adopts the following technical scheme to achieve the above-mentioned purpose:

[0005] A preparation method of a spinel carbon material with a low thermal expansion rate, the preparation method comprising: pre-treating spinel particles, namely, mixing the spinel particles with one of wax, silica sol and PVA to form a thin film on the surface of the spinel particles; the amount of wax, silica sol and PVA added is 1-5% of the spinel particles; drying the mixed spinel raw material; taking 45% of the pre-treated spinel particles, 15% of flake graphite, 35% of 200-mesh spinel fine powder and 5% of phenolic resin by mass percentage, mixing in a mixer to form a spinel carbon raw material, drying at 60°C for 6h, cold isostatic pressing under a pressure of 100Mpa, and heat treating at 950°C for 5h to prepare a spinel carbon material with a low thermal expansion rate.

[0006] The spinel particles are one of fused spinel and sintered spinel.

[0007] The wax is one of paraffin and beeswax; when using the wax, it needs to be melted into liquid first.

[0008] The spinel particles have a particle size of 1-0.2 mm.

[0009] The invention provides a method for preparing a spinel carbon material with a low thermal expansion rate, wherein one of wax, silica sol and PVA is mixed with spinel particles. After the mixing is completed, a thin film is formed on the surface of the spinel particles, and then the raw materials treated by the method are used to prepare spinel carbon products. The heat treatment temperature of the spinel carbon products is above 900°C. During the heat treatment process, the wax or PVA on the surface of the spinel particles disappears, and a circle of fine gaps is formed on the surface of the spinel particles, while the silica sol forms a large number of holes on the surface of the spinel particles. These gaps or holes offset the thermal expansion of the spinel material during use, thereby reducing the thermal expansion rate of the spinel carbon material product. According to the relevant theories of thermal shock fracture resistance and thermal shock damage resistance of materials, the thermal expansion rate of the material is the main factor affecting its thermal shock resistance. The smaller the thermal expansion rate of the refractory material, the better the thermal shock resistance. DETAILED DESCRIPTION

[0010] The present invention is described in detail with reference to specific embodiments: Embodiment 1:

[0011] Weigh 100 parts of fused spinel (1-0.2 mm) and 1 part of paraffin by mass. Melt the paraffin at 90° C. into liquid, mix in a mixer for 10 minutes, and dry naturally in air for 2 hours. Weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of fused spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix in a mixer to form a spinel carbon raw material, dry at 60° C. for 6 hours, cold isostatically press under a pressure of 100 MPa, and heat treat at 950° C. for 5 hours to make a spinel carbon product. Embodiment 2:

[0012] Weigh 100 parts of sintered spinel (1-0.2 mm) and 3 parts of paraffin wax by mass. Melt the paraffin wax into liquid at 90°C, mix in a mixer for 10 minutes, and dry naturally in air for 2 hours. Weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of sintered spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix in a mixer to form a spinel carbon raw material, dry at 60°C for 6 hours, cold isostatically press under a pressure of 100 MPa, and heat treat at 950°C for 5 hours to make a spinel carbon product. Embodiment 3:

[0013] Weigh 100 parts of fused spinel (1-0.2 mm) and 5 parts of paraffin wax by mass. Melt the paraffin wax at 90° C. into liquid, mix in a mixer for 10 minutes, and dry naturally in air for 2 hours. Weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of fused spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix in a mixer to form a spinel carbon raw material, dry at 60° C. for 6 hours, cold isostatically press under a pressure of 100 MPa, and heat treat at 950° C. for 5 hours to make a spinel carbon product. Embodiment 4:

[0014] Weigh 100 parts of sintered spinel (1-0.2 mm) and 1 part of beeswax by mass. Melt the beeswax at 90° C. into liquid, mix in a mixer for 10 minutes, and dry naturally in air for 2 hours. Weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of sintered spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix in a mixer to form a spinel carbon raw material, dry at 60° C. for 6 hours, cold isostatically press under a pressure of 100 MPa, and heat treat at 950° C. for 5 hours to make a spinel carbon product. Embodiment 5:

[0015] Weigh 100 parts of fused spinel (1-0.2 mm) and 3 parts of beeswax by mass, melt the beeswax at 90°C into liquid, mix in a mixer for 10 minutes, and dry naturally in air for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of fused spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix in a mixer to form a spinel carbon raw material, dry at 60°C for 6 hours, cold isostatically press under a pressure of 100 MPa, and heat treat at 950°C for 5 hours to make a spinel carbon product. Embodiment 6:

[0016] Weigh 100 parts of sintered spinel (1-0.2 mm) and 5 parts of beeswax by mass, melt the beeswax at 90°C into liquid, mix in a mixer for 10 minutes, and dry naturally in air for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of sintered spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix in a mixer to form a spinel carbon raw material, dry at 60°C for 6 hours, cold isostatically press under a pressure of 100Mpa, and heat treat at 950°C for 5 hours to make a spinel carbon product. Embodiment 7:

[0017] Weigh 100 parts of fused spinel (1-0.2 mm) and 1 part of silica sol by mass, mix them in a mixer for 10 minutes, and dry them at 60°C for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of fused spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix them in a mixer to form a spinel carbon raw material, dry them at 60°C for 6 hours, cold isostatically press them under a pressure of 100 MPa, and heat treat them at 950°C for 5 hours to make spinel carbon products. Embodiment 8:

[0018] Weigh 100 parts of fused spinel (1-0.2 mm) and 3 parts of silica sol by mass, mix them in a mixer for 10 minutes, and dry them at 60°C for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of fused spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix them in a mixer to form a spinel carbon raw material, dry them at 60°C for 6 hours, cold isostatically press them under a pressure of 100 MPa, and heat treat them at 950°C for 5 hours to make spinel carbon products. Embodiment 9:

[0019] Weigh 100 parts of sintered spinel (1-0.2 mm) and 5 parts of silica sol by mass, mix them in a mixer for 10 minutes, and dry them at 60°C for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of sintered spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix them in a mixer to form a spinel carbon raw material, dry them at 60°C for 6 hours, cold isostatically press them under a pressure of 100 MPa, and heat treat them at 950°C for 5 hours to make spinel carbon products.

[0020] Embodiment 10:

[0021] Weigh 100 parts of sintered spinel (1-0.2 mm) and 1 part of PVA by mass, mix them in a mixer for 10 minutes, and dry them at 60°C for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of sintered spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix them in a mixer to form a spinel carbon raw material, dry them at 60°C for 6 hours, cold isostatically press them under a pressure of 100 MPa, and heat treat them at 950°C for 5 hours to make spinel carbon products.

[0022] Embodiment 11:

[0023] Weigh 100 parts of fused spinel (1-0.2 mm) and 3 parts of PVA by mass, mix them in a mixer for 10 minutes, and dry them at 60°C for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of fused spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix them in a mixer to form a spinel carbon raw material, dry them at 60°C for 6 hours, cold isostatically press them under a pressure of 100 MPa, and heat treat them at 950°C for 5 hours to make spinel carbon products.

[0024] Embodiment 12:

[0025] Weigh 100 parts of sintered spinel (1-0.2 mm) and 5 parts of PVA by mass, mix them in a mixer for 10 minutes, and dry them at 60°C for 2 hours; weigh 45 parts of the above-treated spinel particles, 15 parts of flake graphite, 35 parts of sintered spinel fine powder (200 mesh), and 5 parts of phenolic resin, mix them in a mixer to form a spinel carbon raw material, dry them at 60°C for 6 hours, cold isostatically press them under a pressure of 100 MPa, and heat treat them at 950°C for 5 hours to make spinel carbon products.

[0026] At the same time, in order to compare the effects of the present invention, a comparative sample was prepared.

[0027] Comparative sample 1: 45 parts of sintered spinel particles, 15 parts of flake graphite, 35 parts of sintered spinel fine powder (200 mesh), and 5 parts of phenolic resin are mixed in a mixer to form spinel carbon raw materials, dried at 60°C for 6 hours, cold isostatically molded under a pressure of 100 MPa, and heat treated at 950°C for 5 hours to make spinel carbon products.

[0028] Comparative sample 2: 45 parts of fused spinel particles, 15 parts of flake graphite, 35 parts of fused spinel fine powder (200 mesh), and 5 parts of phenolic resin are mixed in a mixer to form spinel carbon raw materials, dried at 60°C for 6 hours, cold-pressed under a pressure of 100 MPa, and heat treated at 950°C for 5 hours to make spinel carbon products.

[0029] The thermal expansion coefficients of various schemes in the range of room temperature to 1300°C are shown in Table 1.

[0030] Table 1 Thermal expansion rate of each solution (%)

[0031] .

Claims

1. A method for preparing a low thermal expansion spinel carbon material, characterized in that: The preparation method is as follows: pre-treating spinel particles, that is, mixing the spinel particles with one of wax, silica sol and PVA to form a thin film on the surface of the spinel particles; the amount of wax, silica sol and PVA added is 1-5% of the spinel particles; the particle size of the spinel particles is 0.2-1mm; drying the mixed spinel particles; taking 45% of the pre-treated spinel particles, 15% of flake graphite, 35% of 200-mesh spinel fine powder and 5% of phenolic resin by mass percentage, mixing them in a mixer to form a spinel carbon raw material, drying at 60°C for 6h, cold isostatic pressing under a pressure of 100Mpa, and heat treating at 950°C for 5h to prepare a spinel carbon material with a low thermal expansion coefficient.

2. The method for preparing a low thermal expansion spinel carbon material according to claim 1, characterized in that: The spinel particles are one of fused spinel and sintered spinel.

3. The method for preparing a low thermal expansion spinel carbon material according to claim 1, characterized in that: The wax is one of paraffin and beeswax; when using the wax, it needs to be melted into liquid first.