A kind of plugging cement-based gelling material for cementing and preparation method thereof

By using composite materials of fast hard sulfaluminate cement and granulated blast furnace slag in the plugging agent, combined with quartz sand and treated composite fibers, the problems of high cost of existing plugging agents and environmental pollution are solved, and the problem of high cost of existing plugging agents is achieved. Highly efficient cement-based cementitious material has the effect of plugging leakage with high early strength, strong retention and excellent temperature and durability, and meets the goals of energy conservation and environmental protection and solid waste utilization.

CN116716088BActive Publication Date: 2024-11-05JIAHUA SPECIAL CEMENT
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202310588672.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-05
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The existing leak plugging agents are costly and have strong environmental pollution. They ignore the leak plugging performance of the cement substrate itself, and cannot maintain the strength of cement stone and the leak plugging effect under medium and low temperature conditions in high temperature environments.

Method used

Using composite cementitious materials, including a mixture of fast hard sulfaluminate cement and granulated blast furnace slag, combined with quartz sand and composite fibers, the fiber surface is softened and laser treated to increase the toughness of the fiber and the cementitious strength with the matrix, and Use coated silicone and strength decayers to form efficient cement-based gelling materials.

Benefits of technology

It has achieved high early strength, strong retention and excellent temperature resistance of cement-based cementitious materials, reduced pulping costs, reduced environmental pollution, met the leakage plugging needs under high temperature and medium and low temperature conditions, and is in line with energy-saving Environmental protection and solid waste utilization goals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004244475060000141
    Figure BDA0004244475060000141
  • Figure BDA0004244475060000151
    Figure BDA0004244475060000151
  • Figure BDA0004244475060000152
    Figure BDA0004244475060000152
Patent Text Reader

Abstract

The present invention discloses a cement-based cementitious material for plugging leaks for cementing and a preparation method thereof. The cement-based cementitious material for plugging leaks for cementing is composed of the following components by weight: 100 parts of composite cementitious material, 15 to 40 parts of quartz sand, 0.1 to 6 parts of composite fiber, 3 to 10 parts of sedimentation stabilizer, and 1 to 5 parts of anti-strength decay agent. The present invention aims to solve the problems of high manufacturing cost, strong environmental pollution and neglect of the plugging of cement substrate itself in existing plugging agents. The prepared cement-based cementitious material for plugging leaks for cementing has high early strength of its own matrix, strong retention, good plugging performance, excellent heat resistance and durability, and can also use existing solid waste materials to achieve efficient plugging, thereby achieving the purpose of energy saving, environmental protection and solid waste utilization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydraulic cementing materials for oil and gas well cementing, and in particular relates to a plugging cement-based cementing material for cementing and a preparation method thereof. Background Art

[0002] During the drilling and completion process, since the existing technology cannot accurately predict the bearing capacity of the underground rock formation and the development of fracture pores, fluid working fluid often leaks when passing through leaky layers. The leakage directly affects the construction progress and increases the mining cost. It has always been a problem that is of great concern and difficult to solve efficiently in major oil fields. Therefore, the importance of leak prevention and plugging is self-evident. In order to prevent malicious leakage, the plugging methods are roughly divided into: bridging plugging, inorganic gel plugging, polymer plugging and composite material plugging, etc. In the existing technology:

[0003] CN101857800A discloses a cement slurry for cementing and a preparation method thereof, wherein the cement slurry for cementing mainly comprises cement, hemp fiber pretreated with alkali, common admixtures and other components. The invention mainly utilizes the change in surface energy of modified hemp fiber and the enhancement of chemical bonding, as well as the three-dimensional network structure formed on the surface of pores and cracks and cement particles to form a dense filter cake to achieve the purpose of plugging. The invention method can achieve a certain effect on fracture leakage, but does not consider the strength decay of cement stone at high temperature and the anti-pollution problem of cement slurry.

[0004] CN107418533A discloses a thermal well sealing agent, sealing slurry and sealing method, wherein the thermal well sealing agent is composed of oil well cement, slag powder, bentonite, stabilizer and plugging agent. The invention mainly utilizes the stabilizer and the plugging agent to generate a hydration product of high temperature resistant fibrous crystals by secondary reaction, and forms a firm mesh structure in the plugging layer, thereby achieving plugging. The invention method can ensure the strength of cement stone under high temperature and high pressure environment while achieving good plugging effect, but does not consider the retention capacity of the slurry and the plugging effect under medium and low temperature conditions.

[0005] CN112391152A discloses a cementing plugging material and its preparation method and application. The cementing plugging material is composed of a thermosensitive polymer, a polyvinyl alcohol film, a paraffin film, etc. The preparation method is to coat the thermosensitive polymer for the first time with a mixture of polyvinyl alcohol and water as a solution, and then coat the thermosensitive polymer with the polyvinyl alcohol film for the second time with paraffin. The invention can effectively delay the expansion time of the thermosensitive polymer after reaching the temperature sensitive point in the plugging agent, and realize a controllable release time of 10-100 minutes. Since the existing technology cannot accurately predict the actual temperature downhole, the invention does not consider the influence of temperature volatility on the expansion time of the plugging material.

[0006] CN111285642A discloses a plugging agent, a preparation method and its application, wherein the plugging agent is composed of consolidable quartz sand (thermosetting resin treatment), a coagulant, a latex polymer, a sheet material, a fiber material, an oil well cement, etc. The invention utilizes inorganic materials and organic polymers to improve the retention capacity and suspension stability of the slurry in the leakage layer to achieve the purpose of plugging. The invention method does not consider the effective dispersion of the fiber and the heat resistance and durability of the organic polymer. In addition, the cost of the organic polymer is relatively high, making it difficult to promote it widely.

[0007] In summary, the plugging methods currently used mainly improve the performance of cement slurry by adjusting admixtures to meet the plugging requirements, while the cement matrix itself does not play a big role. Some inorganic and organic admixtures have high manufacturing costs and cause great environmental pollution, which are not suitable for the current purpose of energy conservation, environmental protection and solid waste utilization. Summary of the invention

[0008] In order to overcome the defects and shortcomings in the above-mentioned prior art, the present invention provides a cement-based cementitious material for cementing and a preparation method thereof. The purpose of the present invention is to solve the problems of high manufacturing cost, strong environmental pollution and neglect of the cement substrate itself in the existing plugging agent. The plugging cement-based cementitious material of the present invention has high early strength of its own matrix, strong retention, good plugging performance, excellent heat resistance and durability, and uses existing solid waste materials to achieve efficient plugging, thereby achieving the purpose of energy saving, environmental protection and solid waste utilization.

[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0010] A plugging cement-based gelling material for cementing, comprising the following components by weight: 100 parts of composite gelling material, 15-40 parts of quartz sand, 0.1-6 parts of composite fiber, 3-10 parts of sedimentation stabilizer, and 1-5 parts of anti-strength decay agent;

[0011] The composite cementitious material is a mixture of rapid hardening sulphoaluminate cement and granulated blast furnace slag, wherein the mass ratio of rapid hardening sulphoaluminate cement to granulated blast furnace slag is (15-35): (65-85).

[0012] In some embodiments of the present invention, the plugging cement-based cementitious material for cementing includes the following components in parts by weight: 100 parts of composite cementitious material, 30-35 parts of quartz sand, 0.1-6 parts of composite fiber, 5-7 parts of sedimentation stabilizer, and 2-3 parts of anti-strength decay agent;

[0013] Preferably, in the composite cementitious material, the mass ratio of rapid-hardening sulphoaluminate cement: granulated blast furnace slag is (20-35): (65-80).

[0014] Furthermore, the quick-hardening sulphoaluminate cement has Al2O3≥33wt.%, SiO2≤8.5wt.%, and a specific surface area of ​​the quick-hardening sulphoaluminate cement≥360m 2 / kg;

[0015] The granulated blast furnace slag is alkaline slag, and the components of the slag are CaO≥45wt.%, SiO2≥25wt.%, 10wt.%≤Al2O3≤20wt.%, the mass coefficient K>2.4, and the powder particle size D(10)≤2μm, D(50)≤8μm, and D(90)≤22μm.

[0016] Furthermore, the composition of the quartz sand is SiO2≥98wt.%, and the powder fineness of the quartz sand is 100 mesh≤400 mesh.

[0017] The high silica content in quartz sand is used to ensure the calcium-silicon ratio of the cement slurry system and the compressive strength of the cement paste in high temperature environments.

[0018] Furthermore, the composite fiber is a mixture of apocynum fiber, abaca fiber, bamboo fiber and coconut shell fiber;

[0019] Preferably, in terms of mass ratio, apocynum fiber: abaca fiber: bamboo fiber: coconut shell fiber = 1:1:1:1;

[0020] Preferably, the lengths of the apocynum fiber, abaca fiber, bamboo fiber, and coconut shell fiber are L1, L2, L3, and L4, respectively, and L1, L2, L3, and L4 are all greater than or equal to 1 mm and less than or equal to 12 mm;

[0021] More preferably, L1, L2, L3, and L4 are not equal to each other, and the difference between any two of them is ≥3 mm and ≤9 mm.

[0022] Furthermore, the composite fiber is obtained by the following surface treatment:

[0023] (1) Softening treatment: soak the composite fiber in a sodium sulfite solution, then soak it in deionized water, and then dry it;

[0024] Preferably, the temperature of the sodium sulfite solution is 35-50°C, more preferably 45°C, and the concentration of the sodium sulfite solution is 25wt%-30wt%;

[0025] Preferably, the temperature of the deionized water in step (1) is room temperature;

[0026] Preferably, the soaking time in the sodium sulfite solution is 0.5-5h, more preferably 2h;

[0027] Preferably, the soaking time in deionized water in step (1) is 0.5-4 h, more preferably 1 h;

[0028] Preferably, the composite fiber soaked in deionized water in step (1) is dried under vacuum conditions;

[0029] (2) Laser treatment: the composite fiber after the softening treatment in step (1) is placed in the laser vacuum generator in the laser micro-hole punching machine, the airflow hanger is started to evenly disperse the fiber in the vacuum focused by the laser, and then the laser emitter is turned on to perform groove focusing heat treatment on the fiber surface. By emitting laser beams of different diameters and controlling the emission frequency and focusing time of each laser beam, grooves of different diameters and depths are obtained. The treated fiber is then immersed in deionized water and then dried;

[0030] Preferably, the temperature of the deionized water in step (2) is room temperature;

[0031] Preferably, the soaking time in deionized water in step (2) is 10-120 min, more preferably 30 min;

[0032] Preferably, the composite fibers soaked in deionized water in step (2) are dried under vacuum conditions; the drying temperature is 20-30°C, more preferably 27°C.

[0033] The laser treatment process in step (2) is carried out by a laser micro-hole punching machine, which is a precision laser equipment that can provide 1-300 μm laser micro-holes, micro-grooves, cutting, feature molding and other functions. The vacuum generator and the airflow hanger are both internal components of the laser micro-hole punching machine. The laser micro-hole punching machine is directly purchased and used on the market, such as the laser micro-hole FM series customized equipment produced by Fermi Laser Company and the laser drilling customized equipment produced by Yuchang Laser Company. The purpose of the surface treatment of the composite fiber is: first, to remove the lignin on the fiber surface, soften the overall rigidity of the fiber, so that its toughness and strength develop in a coordinated manner; second, the fiber surface with different grooves can greatly increase the roughness and form a stable bond with the matrix, improve the strength and toughness of the cement stone, and at the same time enhance the dense plugging degree of the matrix bonding layer. In some embodiments of the present invention, the diameter and depth of the holes punched on the surface of the composite fiber can be different or not completely the same, and the laser beam diameter and the emission frequency and focusing time of each laser beam are reasonably set according to the specific implementation scheme.

[0034] Furthermore, the sedimentation stabilizer is a mixture of coated micro-silicon and hydroxypropyl methylcellulose;

[0035] Preferably, in terms of mass ratio, the coating micro-silicon:hydroxypropyl methylcellulose=(90-95):(5-10);

[0036] Preferably, the molecular weight of the hydroxypropyl methylcellulose is at the industrial molecular level of 200,000, the SiO2 content of the coated micro-silicon is ≥ 90wt.%, and the powder particle size D(90) is < 8μm.

[0037] Furthermore, the coated micro-silicon is obtained by the following surface treatment: adding micro-silicon powder to the coating solution, mixing and reacting, and vacuum drying to obtain the coated micro-silicon; preferably, the reaction time is 5 to 30 minutes; more preferably 10 minutes;

[0038] The coating solution is composed of anhydrous ethanol, cross-linked polyvinyl pyrrolidone, dibutyl sebacate, and dimethyl phthalate, wherein the mass ratio of anhydrous ethanol: cross-linked polyvinyl pyrrolidone: dibutyl sebacate: dimethyl phthalate is (60-75): (5-10): (10-15): (10-15)

[0039] Preferably, the vacuum drying temperature is 30 to 50°C, more preferably 40°C;

[0040] Preferably, the concentration of the coating solution is 60wt.% to 90wt.%;

[0041] Preferably, the usage ratio of microsilica powder to plating solution is 1:(10-200).

[0042] The purpose of coating the microsilica powder is that: microsilica powder with finer particle size will thicken significantly during the cement slurry preparation process, making it difficult to quickly deposit and not conducive to on-site construction; after the coating treatment, a layer of plastic resin protective film is formed on the surface of the microsilica, which can effectively prevent the microsilica from reacting with water under low temperature conditions. At this time, the coated microsilica is evenly dispersed in the cement slurry as a filling material. As the temperature rises during the grouting process, the resin protective film begins to decompose, and the microsilica begins to absorb water and expand, continuously enhancing the molecular surface viscosity and increasing the slurry viscosity, thereby preventing high-temperature sedimentation of large solid particles.

[0043] The working principle of the sedimentation stabilizer is as follows: during the pulping process, hydroxypropyl methylcellulose is mainly used for viscosity enhancement and anti-settling, and the coated microsilica at this time does not affect the fluidity of the slurry; during the grouting process, as the temperature continues to rise, the hydroxypropyl methylcellulose molecular chain begins to decompose and fail, and the viscosity-enhancing effect decreases. At this time, the resin protective film on the surface of the coated microsilica also begins to decompose and destroy, and the microsilica expands when it meets water, continuously increasing the molecular surface viscosity, gradually increasing the slurry viscosity, and preventing the solid phase particles from settling. During the whole process, hydroxypropyl methylcellulose and the coated microsilica are reasonably matched to control the suspension stability of the cement slurry in the entire temperature range.

[0044] Furthermore, the anti-strength decay agent is a mixture of dihydrate gypsum, green vitriol and sulfuric acid mud;

[0045] Preferably, in terms of mass ratio, dihydrate gypsum: green vitriol: sulfate mud = (70-80): (10-20): (5-10);

[0046] Preferably, the composition of CaSO4·2H2O in the dihydrate gypsum is ≥99wt.%; the composition of FeSO4·7H2O in the green vitriol is ≥95wt.%; the composition of Fe2(SO4)3 in the sulfate mud is ≥95wt.%, and the powder fineness of the sulfate mud is ≥600 mesh.

[0047] The working principle of the anti-strength decay agent is as follows: first, the ferrous sulfate aqueous solution in green vitriol easily forms a hexahydrated complex salt with the calcium ions in the cement slurry, and the ferrous sulfate complex salt is wrapped on the surface of the high-temperature hydration product tobermorite. The complex salt robs the calcium ions and hinders the contact between tobermorite and other mineral ions. The high-temperature stability of the complex salt not only improves the crystal stability of tobermorite at high temperature, but also prevents tobermorite from transforming into xonotlite, thereby improving the performance of cement paste in resisting high-temperature strength decay; second, ettringite is a major hydration product of sulphoaluminate cement and granulated blast furnace slag. By increasing the sulfate ion concentration in the cement slurry, the transformation of ettringite to monosulfur hydrated calcium sulphoaluminate at high temperature is inhibited, thereby improving the thermal stability of ettringite and ensuring that the strength of cement paste does not decay in a high-temperature environment.

[0048] The present invention also provides a method for preparing a cement-based cementitious material for plugging leaks for cementing, comprising the following steps:

[0049] Step A, initially mixing the fiber and the slag: adding water to the granulated blast furnace slag to form a slag working liquid, stirring the slag working liquid at a low speed while uniformly adding the composite fiber to obtain a uniformly mixed fiber-slag working liquid, and vacuum drying the uniformly mixed fiber-slag working liquid to obtain a fiber-slag mixed powder;

[0050] Preferably, the mass ratio of granulated blast furnace slag to water is (65-85):(100-200);

[0051] Preferably, the mass ratio of granulated blast furnace slag to composite fiber is (65-85):(0.1-6);

[0052] Preferably, the vacuum drying temperature is 40 to 60°C;

[0053] Step B, secondary mixing of the fiber-slag mixed powder and other materials: the fiber-slag mixed powder, rapid hardening sulphoaluminate cement, quartz sand, sedimentation stabilizer and strength decay resistance agent are mixed evenly in a mixer to obtain a plugging cement-based cementitious material for cementing.

[0054] One of the purposes of the preparation method is to ensure uniform distribution of the fibers in the cement matrix by initially mixing the composite fibers in the solid waste matrix and then mixing the mixture with other materials for a second time.

[0055] Compared with the prior art, the present invention has the following beneficial effects:

[0056] (1) The plugging cement-based cementitious material for cementing of the present invention has good compatibility with oilfield admixtures. The settlement stability, thickening time, water loss and free liquid of the cement slurry system formed by the matching meet the requirements of on-site plugging construction. Under curing at 20-180°C, the plugging pressure of the cement stone reaches more than 7MPa after 6h plugging and the compressive strength does not decline after 28d.

[0057] (2) The plugging cement-based cementitious material for cementing of the present invention relies on the cement matrix itself to plug leaks. The formed cement slurry has strong retention in cracks, the cement stone matrix has high early strength and good plugging properties. It not only realizes the recycling of existing solid waste materials, but also the inorganic admixtures used are pollution-free to the environment, thereby achieving the purpose of energy conservation, emission reduction and solid waste utilization.

[0058] (3) The cement-based cementitious material for plugging leaks in cementing of the present invention not only has the characteristic of rapid early strength development, but also has the advantage of low hydration heat release, which can effectively reduce the hydration heat release peak and total heat release of cement slurry, thereby improving the self-volume stability of cement stone during solidification and preventing thermal stress concentration from causing cement stone cracking.

[0059] (4) The cement-based cementitious material for plugging leaks in the cementing process of the present invention has strong anti-pollution and water-intrusion resistance. The cement stone formed by the slurry has micro-expansion and a strong matrix density, which can not only improve the sealing ability of the cement ring interface, but also has good anti-permeability and anti-sulfate corrosion capabilities. DETAILED DESCRIPTION

[0060] The technical solution of the present invention is described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0061] In the following embodiments, cement slurry is prepared according to GB / T 19139 standard. The admixtures used include a fluid loss reducer, a dispersant, a retarder and a defoamer. The fluid loss reducer is at least one of carboxymethyl hydroxyethyl cellulose, acrylamide-acrylic acid copolymer, and styrene / AMPS copolymer. The dispersant is at least one of polystyrene sulfonate, formaldehyde and acetone condensation product. The retarder is at least one of boric acid, citric acid, tartaric acid, and AMPS / AA copolymer. The defoamer is at least one of organosiloxanes and polyethers.

[0062] Example 1

[0063] As a preferred embodiment of the present invention, a method for preparing a high-efficiency plugging cement-based gelling material for cementing disclosed in this embodiment comprises the following steps:

[0064] Step A, initially mixing the fiber and the slag: 65 parts by weight of granulated blast furnace slag and 100 parts by weight of water are mixed to form a slag working liquid, 1 part by weight of composite fiber is uniformly added at a low speed while the slag working liquid is stirred, and the evenly mixed fiber-slag working liquid is placed in a vacuum drying oven at 45° C. and dried to obtain a fiber-slag mixed powder;

[0065] Step B, secondary mixing of the fiber-slag mixed powder and other materials: 66 parts by weight of the fiber-slag mixed powder, 35 parts by weight of fast-hardening sulphoaluminate cement, 30 parts by weight of quartz sand, 5 parts by weight of a sedimentation stabilizer and 2 parts by weight of an anti-strength decay agent are mixed evenly in a mixer to obtain the cement-based cementitious material for plugging leaks in cementing of this embodiment, referred to as "1# cement".

[0066] The formula of "1# cement slurry system" matching "1# cement" is: 100 parts by weight of "1# cement" + 5 parts by weight of fluid loss reducer (carboxymethyl hydroxyethyl cellulose) + 0.3 parts by weight of dispersant (polystyrene sulfonate) + 2 parts by weight of retarder (boric acid) + 0.1 parts by weight of defoaming agent (organic silicone) + 60 parts by weight of water.

[0067] The quick-hardening sulphoaluminate cement has Al2O3≥33wt.%, SiO2≤8.5wt.% and a specific surface area≥360m 2 / kg; the granulated blast furnace slag is alkaline slag, the composition of the slag is CaO ≥ 45wt.%, SiO2 ≥ 25wt.%, 10wt.% ≤ Al2O3 ≤ 20wt.%, the quality coefficient K>2.4, the powder particle size D(10) ≤ 2μm, D(50) ≤ 8μm, D(90) ≤ 22μm.

[0068] The composition of the quartz sand is SiO2≥98wt.%, and the powder fineness of the quartz sand is 100 mesh≤400 mesh.

[0069] The composite fiber is a mixture of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber, wherein the mass ratio of ramie fiber: abaca fiber: bamboo fiber: coconut shell fiber is 1:1:1:1, and the lengths of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber are 3mm, 6mm, 9mm and 12mm respectively.

[0070] The composite fiber must undergo the following surface treatments: (1) Softening treatment: soak the composite fiber in a sodium sulfite solution at a temperature of 45°C and a concentration of 30wt.% for 2 hours, then soak it in deionized water at 27°C for 1 hour, and finally dry it in a vacuum drying oven at 60°C; (2) Laser treatment: first, place the softened composite fiber into a laser vacuum generator, start the airflow hanger to evenly disperse the fiber in the vacuum focused by the laser, then turn on the laser emitter to perform groove focusing heat treatment on the fiber surface, and by emitting laser beams of different diameters and controlling the emission frequency and focusing time of each laser beam, grooves of different diameters and depths are obtained, then the treated fiber is soaked in deionized water at 27°C for 30 minutes, and finally dried in a vacuum drying oven at 27°C.

[0071] The sedimentation stabilizer is a mixture of coated microsilicon and hydroxypropyl methylcellulose, wherein the mass ratio of coated microsilicon to hydroxypropyl methylcellulose is 90:10, and the molecular weight of the hydroxypropyl methylcellulose is industrial 200,000 molecular grade; the SiO2 content of the coated microsilicon is ≥90wt.%, and the powder particle size D(90) is <8μm;

[0072] The coated micro-silicon is obtained by the following surface treatment: 10 parts by weight of micro-silicon powder is added to 200 parts by weight of a 90wt.% coating solution, mixed evenly and reacted for 10 minutes, and placed in a 40°C vacuum drying oven for drying to obtain the coated micro-silicon; the coating solution is composed of anhydrous ethanol, cross-linked polyvinyl pyrrolidone, dibutyl sebacate, and dimethyl phthalate, wherein, by mass ratio, anhydrous ethanol: cross-linked polyvinyl pyrrolidone: dibutyl sebacate: dimethyl phthalate = 75:5:10:10.

[0073] The anti-strength decay agent is a mixture of dihydrate gypsum, green vitriol and sulfate mud, wherein the mass ratio of dihydrate gypsum: green vitriol: sulfate mud is 70:20:10; the components of the dihydrate gypsum are CaSO4·2H2O≥99wt.%, the components of the green vitriol are FeSO4·7H2O≥95wt.%, the components of the sulfate mud are Fe2(SO4)3≥95wt.%, and the powder fineness is ≥600 mesh.

[0074] Example 2

[0075] As a preferred embodiment of the present invention, a method for preparing a cement-based cementitious material for plugging wells disclosed in this embodiment comprises the following steps:

[0076] Step A, initially mixing the fiber and the slag: 70 parts by weight of granulated blast furnace slag and 120 parts by weight of water are mixed into a slag working liquid, 2 parts by weight of composite fiber is uniformly added while the slag working liquid is stirred at a low speed, and the evenly mixed fiber-slag working liquid is placed in a vacuum drying oven at 40° C. and dried to obtain a fiber-slag mixed powder;

[0077] Step B, secondary mixing of the fiber-slag mixed powder and other materials: 72 parts by weight of the fiber-slag mixed powder, 30 parts by weight of fast-hardening sulphoaluminate cement, 30 parts by weight of quartz sand, 5 parts by weight of a sedimentation stabilizer and 2 parts by weight of an anti-strength decay agent are mixed evenly in a mixer to obtain the cement-based cementitious material for cementing in this embodiment, referred to as "2# cement".

[0078] The formula of "2# cement slurry system" matching "2# cement" is: 100 parts by weight of "2# cement" + 5 parts by weight of fluid loss reducer (carboxymethyl hydroxyethyl cellulose) + 0.3 parts by weight of dispersant (polystyrene sulfonate) + 2 parts by weight of retarder (boric acid) + 0.1 parts by weight of defoaming agent (organic silicone) + 60 parts by weight of water.

[0079] The quick-hardening sulphoaluminate cement has Al2O3≥33wt.%, SiO2≤8.5wt.% and a specific surface area≥360m 2 / kg; the granulated blast furnace slag is alkaline slag, the composition of the slag is CaO ≥ 45wt.%, SiO2 ≥ 25wt.%, 10wt.% ≤ Al2O3 ≤ 20wt.%, the quality coefficient K>2.4, the powder particle size D(10) ≤ 2μm, D(50) ≤ 8μm, D(90) ≤ 22μm.

[0080] The composition of the quartz sand is SiO2≥98wt.%, and the powder fineness of the quartz sand is 100 mesh≤400 mesh.

[0081] The composite fiber is a mixture of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber, wherein the mass ratio of ramie fiber: abaca fiber: bamboo fiber: coconut shell fiber is 1:1:1:1, and the lengths of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber are 3mm, 6mm, 9mm and 12mm respectively.

[0082] The composite fiber must undergo the following surface treatments: (1) softening treatment: soak the composite fiber in a sodium sulfite solution at a temperature of 35°C and a concentration of 30wt.% for 5 hours, then soak it in deionized water at 27°C for 0.5 hours, and finally dry it in a vacuum drying oven at 60°C; (2) laser treatment: first put the softened composite fiber into a laser vacuum generator, then start the airflow hanger to evenly disperse the fiber in the vacuum focused by the laser, then turn on the laser emitter to perform groove focusing heat treatment on the fiber surface, and by emitting laser beams of different diameters and controlling the emission frequency and focusing time of each laser beam, grooves of different diameters and depths are obtained, and then the treated fiber is soaked in deionized water at 27°C for 120 minutes, and finally dried in a vacuum drying oven at 30°C.

[0083] The sedimentation stabilizer is a mixture of coated microsilicon and hydroxypropyl methylcellulose, wherein the mass ratio of coated microsilicon to hydroxypropyl methylcellulose is 90:10, the molecular weight of the hydroxypropyl methylcellulose is industrial 200,000 molecular grade, the SiO2 content of the coated microsilicon is ≥90wt.%, and the powder particle size D(90) is <8μm;

[0084] The coated micro-silicon is obtained by the following surface treatment: 10 parts by weight of micro-silicon powder is added to 100 parts by weight of a coating solution with a concentration of 80wt.%, mixed evenly and reacted for 10 minutes, and placed in a vacuum drying oven at 40°C for drying to obtain the coated micro-silicon; the coating solution is composed of anhydrous ethanol, cross-linked polyvinyl pyrrolidone, dibutyl sebacate, and dimethyl phthalate, wherein, by mass ratio, anhydrous ethanol: cross-linked polyvinyl pyrrolidone: dibutyl sebacate: dimethyl phthalate = 60:10:15:15.

[0085] The anti-strength decay agent is a mixture of dihydrate gypsum, green vitriol and sulfuric acid mud, wherein the mass ratio of dihydrate gypsum: green vitriol: sulfuric acid mud is 80:10:10. The dihydrate gypsum contains CaSO4·2H2O≥99wt.%, the green vitriol contains FeSO4·7H2O≥95wt.%, the sulfuric acid mud contains Fe2(SO4)3≥95wt.%, and the powder fineness is ≥600 mesh.

[0086] Example 3

[0087] As a preferred embodiment of the present invention, a method for preparing a cement-based cementitious material for plugging wells disclosed in this embodiment comprises the following steps:

[0088] Step A, initial mixing of fiber and slag: 75 parts by weight of granulated blast furnace slag and 140 parts by weight of water are mixed to form a slag working liquid, 3 parts by weight of composite fiber are added at a uniform speed while the slag working liquid is stirred at a low speed, and the evenly mixed fiber-slag working liquid is placed in a vacuum drying oven at 60° C. for drying to obtain a fiber-slag mixed powder;

[0089] Step B, secondary mixing of the fiber-slag mixed powder and other materials: 78 parts by weight of the fiber-slag mixed powder, 25 parts by weight of fast-hardening sulphoaluminate cement, 35 parts by weight of quartz sand, 7 parts by weight of a sedimentation stabilizer and 3 parts by weight of an anti-strength decay agent are mixed evenly in a mixer to obtain the cement-based cementitious material for plugging leaks in cementing of this embodiment, referred to as "3# cement".

[0090] The formula of "3# cement slurry system" matching "3# cement" is: 100 parts by weight of "3# cement" + 6 parts by weight of fluid loss reducer (carboxymethyl hydroxyethyl cellulose) + 0.5 parts by weight of dispersant (polystyrene sulfonate) + 3 parts by weight of retarder (boric acid) + 0.1 parts by weight of defoaming agent (organic silicone) + 60 parts by weight of water.

[0091] The quick-hardening sulphoaluminate cement has Al2O3≥33wt.%, SiO2≤8.5wt.% and a specific surface area≥360m 2 / kg, the granulated blast furnace slag is alkaline slag, the components of the slag include CaO≥45wt.%, SiO2≥25wt.%, 10wt.%≤Al2O3≤20wt.%, mass coefficient K>2.4, and the powder particle size is D(10)≤2μm, D(50)≤8μm, and D(90)≤22μm.

[0092] The composition of the quartz sand is SiO2≥98wt.%, and the powder fineness of the quartz sand is 100 mesh≤400 mesh.

[0093] The composite fiber is a mixture of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber, wherein the mass ratio of ramie fiber: abaca fiber: bamboo fiber: coconut shell fiber is 1:1:1:1, and the lengths of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber are 12 mm, 9 mm, 6 mm and 3 mm respectively.

[0094] The composite fiber must undergo the following surface treatments: (1) Softening treatment: soak the composite fiber in a sodium sulfite solution at a temperature of 50°C and a concentration of 30wt.% for 0.5h, then soak it in deionized water at 27°C for 4h, and finally dry it in a vacuum drying oven at 60°C; (2) Laser treatment: first, place the softened composite fiber into a laser vacuum generator, start the airflow hanger to evenly disperse the fiber in the vacuum focused by the laser, then turn on the laser emitter to perform groove focusing heat treatment on the fiber surface, and by emitting laser beams of different diameters and controlling the emission frequency and focusing time of each laser beam, grooves of different diameters and depths are obtained, then the treated fiber is soaked in deionized water at 27°C for 10min, and finally dried in a vacuum drying oven at 27°C.

[0095] The sedimentation stabilizer is a mixture of coated microsilicon and hydroxypropyl methylcellulose, wherein the mass ratio of coated microsilicon to hydroxypropyl methylcellulose is 95:5, the molecular weight of the hydroxypropyl methylcellulose is industrial 200,000 molecular grade, the SiO2 content of the coated microsilicon is ≥90%, and the powder particle size D(90) is <8 μm;

[0096] The coated micro-silicon is obtained by the following surface treatment: 10 parts by weight of micro-silicon powder is added to 2000 parts by weight of a coating solution with a concentration of 60wt.%, mixed evenly and reacted for 10 minutes, and placed in a vacuum drying oven at 40°C for drying to obtain the coated micro-silicon; the coating solution is composed of anhydrous ethanol, cross-linked polyvinyl pyrrolidone, dibutyl sebacate, and dimethyl phthalate, wherein, by mass ratio, anhydrous ethanol: cross-linked polyvinyl pyrrolidone: dibutyl sebacate: dimethyl phthalate = 65:10:10:15.

[0097] The anti-strength decay agent is a mixture of dihydrate gypsum, green vitriol and sulfuric acid mud, wherein the mass ratio of dihydrate gypsum: green vitriol: sulfuric acid mud is 75:15:10. The components of the dihydrate gypsum are CaSO4·2H2O≥99wt.%, the components of the green vitriol are FeSO4·7H2O≥95wt.%, the components of the sulfuric acid mud are Fe2(SO4)3≥95wt.%, and the powder fineness is ≥600 mesh.

[0098] Example 4

[0099] As a preferred embodiment of the present invention, a method for preparing a cement-based cementitious material for plugging wells disclosed in this embodiment comprises the following steps:

[0100] Step A, initially mixing the fiber and the slag: 80 parts by weight of slag and 160 parts by weight of water are mixed to form a slag working solution, 4 parts by weight of composite fiber are added at a uniform speed while the slag working solution is stirred at a low speed, and the evenly mixed fiber-slag working solution is placed in a vacuum drying oven at 45° C. for drying to obtain a fiber-slag mixed powder;

[0101] Step B, secondary mixing of the fiber-slag mixed powder and other materials: 84 parts by weight of the fiber-slag mixed powder, 20 parts by weight of fast-hardening sulphoaluminate cement, 35 parts by weight of quartz sand, 7 parts by weight of a sedimentation stabilizer and 3 parts by weight of an anti-strength decay agent are mixed evenly in a mixer to obtain the high-efficiency plugging cement-based cementitious material for cementing of the embodiment, referred to as "4# cement".

[0102] The formula of "4# cement slurry system" matching "4# cement" is: 100 parts by weight of "4# cement" + 6 parts by weight of fluid loss reducer (carboxymethyl hydroxyethyl cellulose) + 0.5 parts by weight of dispersant (polystyrene sulfonate) + 4 parts by weight of retarder (boric acid) + 0.1 parts by weight of defoaming agent (organic silicone) + 60 parts by weight of water.

[0103] The quick-hardening sulphoaluminate cement has Al2O3≥33wt.%, SiO2≤8.5wt.% and a specific surface area≥360m 2 / kg, the granulated blast furnace slag is alkaline slag, the components of the slag include CaO≥45wt.%, SiO2≥25wt.%, 10wt.%≤Al2O3≤20wt.%, mass coefficient K>2.4, and the powder particle size is D(10)≤2μm, D(50)≤8μm, and D(90)≤22μm.

[0104] The composition of the quartz sand is SiO2≥98wt.%, and the powder fineness of the quartz sand is 100 mesh≤400 mesh.

[0105] The composite fiber is a mixture of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber, wherein the mass ratio of ramie fiber: abaca fiber: bamboo fiber: coconut shell fiber is 1:1:1:1, and the lengths of ramie fiber, abaca fiber, bamboo fiber and coconut shell fiber are 12 mm, 9 mm, 6 mm and 3 mm respectively.

[0106] The composite fiber must undergo the following surface treatments: (1) Softening treatment: soak the composite fiber in a sodium sulfite solution at a temperature of 45°C and a concentration of 30wt.% for 2 hours, then soak it in deionized water at 27°C for 1 hour, and finally dry it in a vacuum drying oven at 60°C; (2) Laser treatment: first, place the softened composite fiber into a laser vacuum generator, start the airflow hanger to evenly disperse the fiber in the vacuum focused by the laser, then turn on the laser emitter to perform groove focusing heat treatment on the fiber surface, and by emitting laser beams of different diameters and controlling the emission frequency and focusing time of each laser beam, grooves of different diameters and depths are obtained, then the treated fiber is soaked in deionized water at 27°C for 30 minutes, and finally dried in a vacuum drying oven at 27°C.

[0107] The sedimentation stabilizer is a mixture of coated microsilicon and hydroxypropyl methylcellulose, wherein the mass ratio of coated microsilicon to hydroxypropyl methylcellulose is 95:5, and further, the molecular weight of the hydroxypropyl methylcellulose is industrial 200,000 molecular grade, the SiO2 content of the coated microsilicon is ≥90wt.%, and the powder particle size D(90) is <8μm;

[0108] The coated micro-silicon is obtained by the following surface treatment: 10 parts by weight of micro-silicon powder is added to 1500 parts by weight of a coating solution with a concentration of 72wt.%, mixed evenly and reacted for 10 minutes, and placed in a vacuum drying oven at 40°C for drying to obtain the coated micro-silicon; the coating solution is composed of anhydrous ethanol, cross-linked polyvinyl pyrrolidone, dibutyl sebacate, and dimethyl phthalate, wherein, by mass ratio, anhydrous ethanol: cross-linked polyvinyl pyrrolidone: dibutyl sebacate: dimethyl phthalate = 70:5:15:10.

[0109] The anti-strength decay agent is a mixture of dihydrate gypsum, green vitriol and sulfuric acid mud, wherein the mass ratio of dihydrate gypsum: green vitriol: sulfuric acid mud is 80:15:5. The components of the dihydrate gypsum are CaSO4·2H2O≥99wt.%, the components of the green vitriol are FeSO4·7H2O≥95wt.%, the components of the sulfuric acid mud are Fe2(SO4)3≥95wt.%, and the powder fineness is ≥600 mesh.

[0110] Comparative Example 1

[0111] Compared with Example 1, the composite fiber in this comparative example is not subjected to surface treatment, and the other conditions are the same. In this comparative example, the apocynum fiber, abaca fiber, bamboo fiber, and coconut shell fiber are directly mixed uniformly according to a certain proportion. The cement-based cementitious material prepared in this comparative example is referred to as "D1# cement".

[0112] The “D1# cement slurry system” that comes with “D1# cement” is the same as the “1# cement slurry system”.

[0113] Comparative Example 2

[0114] Compared with Example 1, the length of the composite fiber in this comparative example is different, and the other conditions are the same. In this comparative example, the lengths of the apocynum fiber, abaca fiber, bamboo fiber, and coconut shell fiber are 15 mm, 12 mm, 9 mm, and 6 mm, respectively.

[0115] The cement-based cementitious material prepared in this comparative example is referred to as "D2# cement".

[0116] The “D2# cement slurry system” that comes with “D2# cement” is the same as the “1# cement slurry system”.

[0117] Comparative Example 3

[0118] Compared with Example 1, the length of the composite fiber in this comparative example is different, and the other conditions are the same. In this comparative example, the lengths of the apocynum fiber, abaca fiber, bamboo fiber, and coconut shell fiber are 12 mm, 9 mm, 4 mm, and 0.5 mm, respectively.

[0119] The cement-based cementitious material prepared in this comparative example is referred to as "D3# cement".

[0120] The “D3# cement slurry system” that comes with “D3# cement” is the same as the “1# cement slurry system”.

[0121] Comparative Example 4 Compared with Example 1, this comparative example uses ordinary micro-silicon instead of coated micro-silicon, and other conditions are the same.

[0122] The cement-based cementitious material prepared in this comparative example is referred to as "D4# cement".

[0123] The “D4# cement slurry system” that comes with “D4# cement” is the same as the “1# cement slurry system”.

[0124] According to the API specification, the engineering properties of the plugging cement-based gelling materials for cementing obtained in Examples 1 to 4 and Comparative Examples 1 to 4 were tested, and the test results are shown in Table 1; according to the Petroleum and Natural Gas Industry Standard SY / T 5840-93 of the People's Republic of China "Indoor Test Methods for Bridging Plug Materials for Drilling", the plugging and leak-proof performance of the cement slurries obtained in Examples 1 to 4 and Comparative Examples 1 to 4 was tested respectively, and the size of the seam plate used was 2×35 mm. The test results are shown in Table 2.

[0125] Table 1 Engineering properties of various cement-based cementitious materials for plugging wells

[0126]

[0127]

[0128] Table 2 Test results of plugging performance of various cement slurries

[0129]

[0130] It can be seen from the engineering performance test results in Table 1 that the plugging cement-based cementitious materials for cementing prepared in Examples 1 to 4 of the present invention have the advantages of zero free liquid, low water loss, good sedimentation stability, linearly adjustable thickening time, and no decline in compressive strength at high temperature. It can be seen from the plugging results in Table 2 that the cement slurry prepared by the plugging cement-based cementitious materials for cementing prepared in the present invention has a small loss of plugging working fluid and an obvious plugging effect.

[0131] Compared with Example 1, the thickening time of the plugging liquid prepared in Example 1 increases, the compressive strength decreases, and the plugging effect is poor, indicating that the composite fiber without softening and laser treatment has a greater influence on the thickening time of the plugging cement slurry, the compressive strength of the plugging cement stone, and the plugging effect. Compared with Example 1, the API water loss of the plugging liquid prepared in Examples 2 and 3 increases, the compressive strength decreases, and the plugging effect becomes worse, indicating that the four fibers in the composite fiber composition need a reasonable gradation relationship in terms of length. The fiber is too long, too short, and the unreasonable gradation relationship will affect the density of the plugging cement and the dispersion of the fiber in the plugging liquid, thereby affecting the API water loss of the plugging cement slurry, the compressive strength of the plugging cement stone, and the plugging effect. Compared with Example 1, the compressive strength of the plugging liquid prepared in Example 4 decreases, and the plugging effect is poor, indicating that the uncoated microsilicon has a greater influence on the strength of the plugging cement stone. In addition, ordinary microsilicon has extremely strong water absorption, which not only makes slurrying difficult, but also affects the plugging effect of the slurry and construction safety.

[0132] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A plugging cement-based gelling material for cementing, characterized in that: The invention comprises the following components by weight: 100 parts of composite cementitious material, 15 to 40 parts of quartz sand, 0.1 to 6 parts of composite fiber, 3 to 10 parts of sedimentation stabilizer, and 1 to 5 parts of anti-strength decay agent; The composite cementitious material is a mixture of rapid hardening sulphoaluminate cement and granulated blast furnace slag, wherein the mass ratio of rapid hardening sulphoaluminate cement to granulated blast furnace slag is (15-35): (65-85); The composite fiber is a mixture of apocynum fiber, abaca fiber, bamboo fiber and coconut shell fiber; In terms of mass ratio, the ratio of apocynum fiber: abaca fiber: bamboo fiber: coconut shell fiber is 1:1:1:1; The lengths of the apocynum fiber, abaca fiber, bamboo fiber and coconut shell fiber are L1, L2, L3 and L4 respectively, and L1, L2, L3 and L4 are all greater than or equal to 1 mm and less than or equal to 12 mm; The composite fiber is obtained by the following surface treatment: (1) Softening treatment: soak the composite fiber in a sodium sulfite solution for 0.5-5 hours, then soak it in deionized water for 0.5-4 hours, and then dry it; the temperature of the sodium sulfite solution is 35-50°C, and the concentration of the sodium sulfite solution is 25wt%-30wt%; (2) Laser treatment: the composite fiber softened in step (1) is placed in a laser vacuum generator in a laser micro-hole punching machine, the airflow hanger is started to evenly disperse the fiber in the laser focused vacuum, and then the laser emitter is turned on to perform groove focusing heat treatment on the fiber surface. By emitting laser beams of different diameters and controlling the emission frequency and focusing time of each laser beam, grooves of different diameters and depths are obtained. The treated fiber is then immersed in deionized water for 10-120 minutes and then dried. The sedimentation stabilizer is a mixture of coated microsilicon and hydroxypropyl methylcellulose; in terms of mass ratio, the coated microsilicon:hydroxypropyl methylcellulose = (90-95): (5-10); the molecular weight of the hydroxypropyl methylcellulose is industrial 200,000 molecular grade, the SiO2 content of the coated microsilicon is ≥90wt.%, and the powder particle size D (90) is <8μm; The coated micro-silicon is obtained by the following surface treatment: adding micro-silicon powder to a coating solution, mixing evenly and reacting for 5 to 30 minutes, and vacuum drying to obtain the coated micro-silicon; The coating solution is composed of anhydrous ethanol, cross-linked polyvinyl pyrrolidone, dibutyl sebacate, and dimethyl phthalate, wherein the mass ratio of anhydrous ethanol: cross-linked polyvinyl pyrrolidone: dibutyl sebacate: dimethyl phthalate is (60-75):(5-10):(10-15):(10-15); the concentration of the coating solution is 60 wt.%-90 wt.%; the usage ratio of microsilica powder to the coating solution is 1:(10-200).

2. The cement-based gelling material for plugging wells according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 100 parts of composite gelling material, 30-35 parts of quartz sand, 0.1-6 parts of composite fiber, 5-7 parts of sedimentation stabilizer and 2-3 parts of anti-strength decay agent.

3. A cement-based gelling material for plugging leaks for cementing according to claim 1 or 2, characterized in that: In the composite cementitious material, the mass ratio of rapid hardening sulphoaluminate cement to granulated blast furnace slag is (20-35):(65-80).

4. A plugging cement-based gelling material for cementing according to claim 1 or 2, characterized in that: The quick-hardening sulphoaluminate cement has Al2O3≥33wt.%, SiO2≤8.5wt.%, and a specific surface area of ​​​​the quick-hardening sulphoaluminate cement of ≥360m 2 / kg; The granulated blast furnace slag is alkaline slag, and the components of the slag are CaO≥45 wt.%, SiO2≥25 wt.%, 10 wt.%≤Al2O3≤20 wt.%, the mass coefficient K>2.4, and the powder particle size is D(10)≤2μm, D(50)≤8μm, and D(90)≤22μm.

5. A plugging cement-based gelling material for cementing according to claim 1 or 2, characterized in that: The composition of the quartz sand is SiO2≥98 wt.%, and the powder fineness of the quartz sand is 100 mesh≤400 mesh.

6. A plugging cement-based gelling material for cementing according to claim 1 or 2, characterized in that: L1, L2, L3, and L4 are not equal to each other, and the difference between them is ≥3mm and ≤9mm.

7. A plugging cement-based gelling material for cementing according to claim 1 or 2, characterized in that: In the step (1), the temperature of the sodium sulfite solution is 45°C; The temperature of the deionized water in step (1) is room temperature; The soaking time in the sodium sulfite solution is 2h; The soaking time in deionized water in step (1) is 1 hour; Drying the composite fiber soaked in deionized water in step (1) under vacuum conditions; The temperature of the deionized water in step (2) is room temperature; The soaking time in deionized water in step (2) is 30 minutes; The composite fiber soaked in deionized water in step (2) is dried under vacuum conditions.

8. The plugging cement-based gelling material for cementing according to claim 7, characterized in that: The drying temperature in step (2) is 20-30°C.

9. The plugging cement-based gelling material for cementing according to claim 7, characterized in that: The drying temperature in step (2) is 27°C.

10. The plugging cement-based gelling material for cementing according to claim 1, characterized in that: Add microsilica powder into the coating solution, mix evenly and react for 10 minutes, and then dry in vacuum at 30-50℃ to obtain coated microsilica.

11. The plugging cement-based gelling material for cementing according to claim 10, characterized in that: After vacuum drying at 40°C, coated micro-silicon was obtained.

12. A plugging cement-based gelling material for cementing according to claim 1 or 2, characterized in that: The anti-strength decay agent is a mixture of dihydrate gypsum, green vitriol and sulfuric acid mud; In terms of mass ratio, dihydrate gypsum: green vitriol: sulfate mud = (70-80): (10-20): (5-10).

13. The plugging cement-based gelling material for cementing according to claim 12, characterized in that: The components of the dihydrate gypsum are CaSO4•2H2O≥99wt.%; the components of the green vitriol are FeSO4•7H2O≥95wt.%; the components of the sulfate mud are Fe2(SO4)3≥95 wt.%, and the powder fineness of the sulfate mud is ≥600 mesh.

14. A method for preparing the cement-based cementitious material for plugging well cementing according to any one of claims 1 to 13, characterized in that: The following steps are involved: Step A, adding water to granulated blast furnace slag to form a slag working liquid, stirring the slag working liquid at a low speed while adding composite fibers at a uniform speed to obtain a uniformly mixed fiber slag working liquid, and then vacuum drying the uniformly mixed fiber slag working liquid to obtain a fiber slag mixed powder; Step B: Evenly mix the fiber slag mixed powder, quick-hardening sulphoaluminate cement, quartz sand, a sedimentation stabilizer and an anti-strength decay agent to obtain a plugging cement-based cementitious material for cementing.

15. The method for preparing the cement-based gelling material for plugging well cementing according to claim 14, characterized in that: The mass ratio of granulated blast furnace slag to water is (65~85):(100~200).

16. The method for preparing the plugging cement-based gelling material for cementing according to claim 14, characterized in that: The mass ratio of granulated blast furnace slag to composite fiber is (65~85):(0.1~6).

17. The method for preparing the plugging cement-based gelling material for cementing according to claim 14, characterized in that: The vacuum drying temperature is 40~60℃.

Citation Information

Patent Citations

  • Leaking stoppage cement slurry for well cementation and preparation method thereof

    CN101857800A

  • Thermal production well cementing agent, cementing slurry and cementing method

    CN107418533A

  • Plugging agent as well as preparation method and application thereof

    CN111285642A

  • Well cementation plugging material and preparation method and application thereof

    CN112391152A

  • Preparation method of efficient plugging waterproof mortar

    CN104743996A