A composite luminescent material and its preparation method and application
By introducing carbon dots and rare earth ions into the fluoride, composite luminescent materials that can be excited by long-wave ultraviolet light are prepared, which solves the problems of lack of types of near-infrared fluorescent materials and a single spectral coverage range, and achieves high luminescence intensity and thermal stability , suitable for multi-field applications.
Patent Information
- Application Number
- CN202310628381.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, there are relatively few types of near-infrared fluorescent materials and a single spectral coverage range, which is difficult to meet the application needs of near-infrared light sources in the fields of ambient light sources, full-spectrum healthy lighting, medical food testing, water quality testing, etc.
A composite luminescent material is used, which consists of carbon dots and fluoride MF2:Ln3+, where M is an alkaline earth metal element and Ln is a rare earth element. It can be excited by long-wave ultraviolet light, emit visible light and near-infrared light, and is prepared by hydrothermal reaction method. , easy to operate, suitable for mass production.
It achieves high luminous intensity and thermal stability within a wide excitation range, can emit visible light and near-infrared light at the same time, has a wide application range, and the preparation method is low in energy consumption and low cost, which is suitable for industrial applications.
Smart Images

Figure CN116716103B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of luminescent materials, and in particular to a composite luminescent material and a preparation method and application thereof. Background Art
[0002] Fluorine-based materials are a common matrix material that generally have lower phonon energy, which can reduce the probability of non-radiative transitions, thereby increasing the rare earth doping ion (Ln 3+ ) and prolongs its energy level lifetime, which is beneficial for energy storage. The SrF2 matrix shows low phonon energy (<350cm -1 ), in 2014, a scholar reported a simple method for preparing pure SrF2 nanoparticles by one-step hydrothermal method. Based on this, a series of Ln 3+ Doped SrF2 materials are studied and developed.
[0003] However, Ln 3+ Due to its low molar absorptivity and narrow absorption band, its luminescence quantum efficiency is low, which seriously restricts the development of its practical application. In order to solve the problem of limited performance of a single material, materials composed of two or more nanomaterials have attracted the interest of researchers. In 2004, when the Scrivens team used the arc discharge method to prepare single-walled carbon nanotubes, they accidentally discovered a fluorescent nanoparticle material. Researchers quickly showed strong interest and expectations in this material. It was not until 2006 that the Sun team further passivated the obtained carbon nanoparticles by laser ablation technology. Nanoparticles with fluorescent properties similar to those previously reported by the Scrivens team were obtained, and the nanoparticles were named carbon dots (CDs). Composite materials doped with carbon dots and rare earth ions can construct a dual-mode luminescent material in the solid state.
[0004] In recent years, the application of near-infrared light sources in the fields of ambient light sources, full-spectrum health lighting, medical and food testing, water quality testing, etc. has become the focus of the industry. However, in the existing technology, the types of near-infrared fluorescent materials are relatively scarce and the spectral coverage is relatively single. Based on this, it is of great significance to develop more near-infrared fluorescent materials. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a composite luminescent material that can be effectively excited by long-wave ultraviolet light and emits visible light and near-infrared light simultaneously.
[0006] The invention also provides a method for preparing the composite luminescent material.
[0007] The present invention also proposes the application of the composite luminescent material.
[0008] According to one aspect of the present invention, a composite luminescent material is provided, wherein the composite luminescent material comprises carbon dots and fluoride, wherein the general formula of the fluoride is MF2:Ln 3+ , wherein M is an alkaline earth metal element; Ln is a rare earth element;
[0009] The composite luminescent material can be excited by ultraviolet light to emit visible light and near-infrared light;
[0010] Wherein, the wavelength of the ultraviolet light is between 320nm and 380nm, and the wavelength of the near-infrared light is between 900nm and 1100nm.
[0011] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the material of the present invention has multiple advantages such as high luminous intensity and good thermal stability. The composite luminescent material can emit both visible light and near-infrared light sources simultaneously under the excitation of light waves within a wider excitation range, and has a wide range of applications.
[0012] In some embodiments of the present invention, the particle size of the composite luminescent material is between 10 nm and 20 nm. The composite luminescent material of the present invention has a small particle size and high crystallinity, which is conducive to the carbon dot→Yb 3+ The energy transfer between them.
[0013] In some embodiments of the present invention, the wavelength of the visible light is between 380 nm and 650 nm.
[0014] In some embodiments of the present invention, the peak value of the near-infrared light is between 950nm and 1050nm.
[0015] In some embodiments of the present invention, the peak value of the near-infrared light is 980 nm.
[0016] In some embodiments of the present invention, the surface of the carbon dots contains at least one of a carboxyl group or an amino group. Carboxyl groups or amino groups are introduced on the surface of the carbon dots to facilitate functionalization, thereby better combining with rare earth ions.
[0017] In some preferred embodiments of the present invention, the alkaline earth metal element is selected from at least one of Ca, Sr or Ba.
[0018] In some more preferred embodiments of the present invention, the rare earth element is selected from at least one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Y or Sc.
[0019] In some preferred embodiments of the present invention, the molar ratio of the rare earth element to the total metal elements (M and Ln) in the composite material is above 1:100, such as greater than 1:100.
[0020] In some preferred embodiments of the present invention, the molar ratio of the rare earth element to the total metal elements (M and Ln) in the composite material is 1 to 5:100.
[0021] In some further embodiments of the present invention, the molar ratio of the rare earth element to the total metal elements (M and Ln) in the composite material is 3:100.
[0022] According to another aspect of the present invention, a method for preparing the composite luminescent material is provided, comprising the following steps: adding an ammonium source and a fluorine source to a mixed solution containing a rare earth metal salt, an alkaline earth metal salt and a metal chelating agent, and preparing the composite luminescent material through a hydrothermal reaction;
[0023] Wherein, the metal chelating agent includes polycarboxylic acid compounds, and all reaction raw materials are soluble substances.
[0024] According to a preferred embodiment of the preparation method of the present invention, there are at least the following beneficial effects: the scheme of the present invention prepares the composite luminescent material by a one-step method, that is, directly adding a soluble ammonium source and a soluble fluorine source to a mixture of a soluble rare earth metal salt, a soluble alkaline earth metal salt and a metal chelator, and synthesizing it by a hydrothermal reaction method. The metal chelator also serves as a carbon dot precursor, and there is no need to add carbon dots. Compared with the traditional synthesis method, which requires first synthesizing carbon dots, synthesizing fluorides, and then adding carbon dots to fluorides to synthesize carbon dot composite luminescent materials, this cumbersome synthesis step, the preparation method of the scheme of the present invention is simple to operate and easy to mass produce.
[0025] The "soluble substance" referred to in the present invention refers to a substance that can dissolve more than 1 gram in 100 grams of water.
[0026] The "hydrothermal reaction" referred to in the present invention refers to a reaction carried out with water as solvent under the condition of heating the reaction system.
[0027] In some embodiments of the present invention, the temperature of the hydrothermal reaction is 150°C to 200°C, such as 160°C, 170°C, 180°C, 190°C, etc.
[0028] The solution of the present invention can be prepared through a low-temperature hydrothermal reaction, has low energy consumption, low production cost, is environmentally friendly, and has good industrial application prospects.
[0029] In some embodiments of the present invention, the hydrothermal reaction time is 3 h to 8 h, such as 4 h, 5 h, 6 h, 7 h, etc.
[0030] The scheme of the invention has short time consumption, high output and good economic benefit.
[0031] In some preferred embodiments of the present invention, during the hydrothermal reaction, the sum of the molar concentrations of rare earth metal ions and alkaline earth metal ions is between 0.05 mol / L and 0.15 mol / L.
[0032] In some preferred embodiments of the present invention, the molar ratio of carboxylate ions in the polycarboxylic acid compound to fluorine in the fluorine source is 0.5 to 2.5:1. By adjusting the content of the polycarboxylic acid compound and the fluorine source, the content of carbon dots is adjusted to achieve Yb 3+ Effective regulation of ion emission intensity can further achieve effective regulation of fluorescence intensity.
[0033] In some preferred embodiments of the present invention, the molar ratio of carboxylate ions in the polycarboxylic acid compound to fluorine in the fluorine source is 6:1.05.
[0034] In some preferred embodiments of the present invention, the polycarboxylic acid compound includes at least one of a polycarboxylic acid and a polycarboxylate.
[0035] In some embodiments of the present invention, the polycarboxylic acid compound is at least one of sodium citrate or potassium citrate.
[0036] In some embodiments of the present invention, the ammonium source and the fluoride source include ammonium fluoride.
[0037] In some embodiments of the present invention, the ammonium source and the fluoride source include a mixture of ammonium chloride and a fluoride salt; the fluoride salt is selected from at least one of ammonium fluoride, sodium fluoride or potassium fluoride.
[0038] In some embodiments of the present invention, the alkaline earth metal salt includes at least one of BaCl2, SrCl2, and CaCl2.
[0039] In some more preferred embodiments of the present invention, the rare earth metal in the soluble rare earth metal salt is preferably at least one of La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Y, and Sc; and the soluble rare earth metal salt is preferably at least one of a rare earth metal nitrate or a rare earth metal hydrochloride.
[0040] In some embodiments of the present invention, the method further comprises stirring before the hydrothermal reaction, so that the reaction materials are mixed more evenly and the reaction rate is higher.
[0041] In some embodiments of the present invention, the stirring temperature is room temperature.
[0042] In some embodiments of the present invention, the stirring time is 1 to 30 minutes.
[0043] In some embodiments of the present invention, the method further comprises a post-treatment operation of the hydrothermal reaction, including centrifugation, washing and drying. No complex purification steps such as recrystallization are required during the post-treatment process, and the raw fluoride is a pure phase.
[0044] In some embodiments of the present invention, the centrifugal speed is 6000 rpm to 12000 rpm.
[0045] In some embodiments of the present invention, the washing is performed using acetone.
[0046] In some embodiments of the present invention, the washing is performed 1 to 3 times.
[0047] In some embodiments of the present invention, the drying is vacuum drying.
[0048] In some embodiments of the present invention, the vacuum drying temperature is 50°C to 100°C.
[0049] In some embodiments of the present invention, the drying time is 8 hours.
[0050] According to another aspect of the present invention, an application of the composite luminescent material is provided, and a light source includes the composite luminescent material.
[0051] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the composite luminescent material of the present invention has high luminescent intensity, and after being excited by ultraviolet light, can simultaneously emit visible light and near-infrared light, and has good application prospects in the fields of visible light sources and near-infrared light sources.
[0052] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0054] Figure 1 Carbon dots / SrF2:Yb prepared in the embodiment of the present invention 3+ (SrF2:Yb 3+ @CDs) composite luminescent material and X-ray diffraction comparison of the carbon dots / SrF2 (SrF2@CDs) prepared in comparative example 1 and the standard hexagonal phase SrF2.
[0055] Figure 2 Carbon dots / SrF2:Yb prepared in the embodiment of the present invention 3+ (SrF2:Yb3+ @CDs) Transmission electron microscope (TEM) images of the composite luminescent material at different magnifications.
[0056] Figure 3 The embodiments of the present invention contain different concentrations of Yb 3+ Carbon dots / SrF2:Yb 3+ Fluorescence emission spectrum of the composite luminescent material.
[0057] Figure 4 The fluorescence emission spectra of comparative example 2 of the present invention containing carbon dots with different concentrations are shown. DETAILED DESCRIPTION
[0058] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. The test methods used in the embodiments are conventional methods unless otherwise specified; the materials, reagents, etc. used, unless otherwise specified, can be reagents and materials obtained from commercial channels. Unless otherwise specified, the same parameter in each embodiment has the same value. The embodiments described below are exemplary and are only used to explain the present invention, and cannot be understood as limitations on the present invention.
[0059] In the description of the present invention, the reference term "between" includes both endpoints.
[0060] The "room temperature" referred to in the present invention refers to 20-30°C, and specifically 25°C in the embodiments.
[0061] Example
[0062] This embodiment prepares a composite luminescent material, and the specific process is as follows:
[0063] S1: Weigh 0.9238g, 0.9145g, 0.9052g, 0.8958g, and 0.8865g of strontium chloride hexahydrate (numbered as strontium chloride samples 1 to 5, respectively), 0.0136g, 0.0271g, 0.0407g, 0.0542g, and 0.0678g of ytterbium chloride hexahydrate (numbered as ytterbium chloride samples 1 to 5, respectively, dissolve the strontium chloride samples and ytterbium chloride samples with the same numbers in 7mL of deionized water, stir them thoroughly until they are completely dissolved, and obtain 5 groups of mixed solutions containing strontium chloride and ytterbium chloride;
[0064] S2: Weigh 5.2938 g of sodium citrate dihydrate, dissolve it in 25 mL of deionized water, and stir thoroughly until it is completely dissolved to prepare 5 sets of the same solution;
[0065] S3: adding the 5 groups of sodium citrate aqueous solutions prepared in S2 to the 5 groups of mixed solutions containing strontium chloride and ytterbium chloride in S1, stirring at 500 r / min for about 8 minutes (5 to 10 minutes) at room temperature to obtain 5 groups of mixed solutions containing sodium citrate, strontium chloride and ytterbium chloride;
[0066] S4: Weigh 0.3500 g of ammonium fluoride, dissolve it in 3 mL of deionized water, and stir thoroughly until it is completely dissolved to prepare 5 sets of the same solution;
[0067] S5: Add the 5 groups of ammonium fluoride solutions in S4 to the 5 groups of mixed solutions in S3, and stir at 500 r / min for about 8 minutes (5 to 10 minutes) at room temperature to obtain 5 groups of mixed solutions containing sodium citrate, strontium chloride, ytterbium chloride and ammonium fluoride;
[0068] S6: placing the five mixed solutions of S5 in an autoclave at 190° C. for reaction for 6 h, and cooling to room temperature after the reaction is completed;
[0069] S7: The obtained product was transferred to a centrifuge tube, centrifuged at 10000 r / min, washed twice with acetone, and ultrasonically treated for 15 min, and dried at 80 °C to obtain Yb 3+ Carbon dots / SrF2:Yb with different doping amounts 3+ Composite luminescent material (SrF2: Yb@CDs), among which Yb 3+ Total metal elements (Sr 2+ and Yb 3+ ) are approximately 1%, 2%, 3%, 4% and 5% in sequence.
[0070] Comparative Example 1
[0071] This comparative example prepares a composite luminescent material, and the specific process is as follows:
[0072] S1: Weigh 0.9332 g of strontium chloride hexahydrate, dissolve it in 7 mL of deionized water, and stir thoroughly until it is completely dissolved;
[0073] S2: Weigh 5.2938 g of sodium citrate dihydrate, dissolve it in 25 mL of deionized water, and stir thoroughly until it is completely dissolved;
[0074] S3: adding the sodium citrate aqueous solution prepared in S2 to the strontium chloride aqueous solution in S1, vigorously stirring at 500 r / min for about 8 minutes (5 to 10 minutes) at room temperature to obtain a mixed solution containing sodium citrate and strontium chloride;
[0075] S4: Weigh 0.3500 g of ammonium fluoride, dissolve it in 3 mL of deionized water, and stir thoroughly until it is completely dissolved;
[0076] S5: adding the ammonium fluoride solution in S4 to the mixed solution in S3, stirring vigorously at 500 r / min for about 8 minutes (5 to 10 minutes) at room temperature to obtain a mixed solution containing sodium citrate, strontium chloride and ammonium fluoride;
[0077] S6: placing the S5 mixed solution in an autoclave at 190°C for reaction for 6 hours, and cooling to room temperature after the reaction is completed;
[0078] S7: The obtained product was transferred to a centrifuge tube, centrifuged at 10000 r / min, washed twice with acetone, and ultrasonically treated for 15 min. The carbon dot / SrF2 composite luminescent material (SrF2@CDs) was obtained by drying at 80°C.
[0079] Comparative Example 2
[0080] This comparative example prepares a composite luminescent material, which differs from comparative example 1 only in the carbon dot content.
[0081] S1: Weigh 0.9332 g of strontium chloride hexahydrate, dissolve it in 7 mL of deionized water, and stir thoroughly until it is completely dissolved;
[0082] S2: Weigh 4.7056 g, 4.9997 g, 5.2938 g, 5.5879 g, 5.8820 g, and 6.4702 g of sodium citrate dihydrate (numbered as strontium chloride samples 1 to 6, respectively), dissolve them in 25 mL of deionized water, and stir them until they are completely dissolved to prepare 6 groups of sodium citrate aqueous solutions with different contents;
[0083] S3: Add the 6 groups of sodium citrate aqueous solutions prepared in S2 to the strontium chloride aqueous solution in S1, and stir vigorously at 500 r / min for about 8 minutes (5 to 10 minutes) at room temperature to obtain 6 groups of mixed solutions containing sodium citrate and strontium chloride;
[0084] S4: Weigh 0.3114 g, 0.3308 g, 0.3500 g, 0.3697 g, 0.3889 g, and 0.4278 g of ammonium fluoride (numbered as strontium chloride samples 1 to 6, respectively), dissolve them in 3 mL of deionized water, and stir them until they are completely dissolved to prepare 6 groups of aqueous solutions of ammonium fluoride with different contents;
[0085] S5: add the 6 groups of ammonium fluoride aqueous solutions in S4 to the mixed solution in S3 in sequence, and stir vigorously at 500 r / min for about 8 minutes (5 to 10 minutes) at room temperature to obtain 6 groups of mixed solutions containing sodium citrate, strontium chloride and ammonium fluoride;
[0086] S6: placing the six mixed solutions in S5 in an autoclave at 190° C. for reaction for 6 h, and cooling to room temperature after the reaction is completed;
[0087] S7: The obtained product is transferred to a centrifuge tube, centrifuged at 10000 r / min, washed twice with acetone, and ultrasonically treated for 15 min. The carbon dot / SrF2 composite luminescent materials with different carbon dot contents are obtained by drying at 80°C.
[0088] Test example
[0089] This test example tests the performance of the composite luminescent materials prepared in the examples and comparative examples.
[0090] 1. X-ray diffraction (XRD) characterization
[0091] The composite luminescent materials prepared in the embodiment and comparative examples 1 to 2 were characterized by X-ray diffraction (XRD) for microstructure characterization. Among them, the XRD graphs of the composite luminescent material with a Yb doping amount of 3% prepared in the embodiment and the composite luminescent material prepared in comparative example 1 are compared with the X-ray diffraction graph of the standard hexagonal phase SrF2 as shown in FIG. Figure 1 As shown. It can be seen from the figure that the diffraction peaks of the composite luminescent materials prepared in the embodiment and comparative example 1 are consistent with the peak positions of the standard card, indicating that the composite luminescent materials prepared in the embodiment and comparative example 1 are in a standard hexagonal phase, are pure phases, and the doping of Yb and carbon dots has no effect on the physical phase. In addition, the peaks of the composite luminescent materials prepared in the embodiment and comparative example 1 are sharp, indicating that the material has high crystallinity. The XRD patterns of the composite luminescent materials with other Yb doping amounts in the embodiments and the composite luminescent materials prepared in comparative example 2 are similar, and are not shown one by one to avoid redundancy.
[0092] 2) Transmission electron microscopy (TEM) characterization
[0093] The microscopic morphology of the composite luminescent materials prepared in the embodiment and the comparative example was characterized, wherein the TEM image of the composite luminescent material prepared in the embodiment is as follows: Figure 2 As shown, Figures (a) and (b) are TEM images at different magnifications. It can be seen from the figure that the particle size of the composite luminescent material is about 15nm, and the particle size of the carbon dots is about 2-5nm. From Figure (b), it can be clearly seen that the orderly lattice structure is arranged, and the lattice spacing is 0.21nm, corresponding to the graphene 100 crystal plane; the lattice spacing is 0.324nm, corresponding to the SrF2 crystal plane, indicating that SrF2 is generated.
[0094] 3) Spectral property characterization
[0095] The emission spectra of the composite luminescent materials prepared in the examples and comparative examples were measured by ultraviolet light excitation. The emission spectra of the composite luminescent materials prepared in the examples under 330 nm ultraviolet light excitation are as follows: Figure 3 As shown, the emission spectrum of the composite luminescent material prepared in Comparative Example 2 under the excitation of 365nm ultraviolet light is as follows Figure 4 shown.
[0096] As can be seen from the figure, Yb doping emits strong near-infrared light with a peak value between 950nm and 1050nm, with a double peak, and the strongest peak is at 980nm. At a doping amount of 1-5%, as the Yb doping amount increases, the luminescence intensity first increases and then decreases. At the same time, the composite luminescent material also emits strong visible light. The wavelength of visible light is between 380nm and 650nm, and the emission wavelength of the emission spectrum of the composite luminescent material in the visible light region is consistent with that of the composite luminescent material without Yb doping.
[0097] In the embodiment of the present invention, the citrate anion serves as a carbon dot precursor and a capping agent, and can also provide a carboxyl group, and NH4F provides an amino group and F - The fluoride preparation process directly contains carbon dots without the need to add additional carbon dots. The composite luminescent material of the present invention can match ultraviolet excitation, has high luminescence intensity, good thermal stability, simple preparation method, short time consumption, low cost, high yield, and is easy to mass produce. CDs and Ln may exist in the composite luminescent material. 3+ The energy transfer process between carbon dots and rare earth luminescent composite materials plays an important role in the luminescence and application of carbon dots and rare earth luminescent composite materials. The scheme of the present invention can provide evidence for the study of the existence of energy transfer and interaction mechanism.
[0098] In addition, the composite luminescent materials prepared by using other alkaline earth metal salts or rare earth metal salts have similar optical properties.
[0099] The embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.
Claims
1. A composite luminescent material, characterized in that: The composite luminescent material comprises carbon dots and fluoride, and the general formula of the fluoride is MF2:Ln 3+ , wherein M is an alkaline earth metal element; Ln is a rare earth element, and the rare earth element is Yb; The composite luminescent material can be excited by ultraviolet light to emit visible light and near-infrared light; Wherein, the wavelength of the ultraviolet light is between 320nm and 380nm, and the wavelength of the near-infrared light is between 900nm and 1100nm; The preparation method of the composite luminescent material comprises the following steps: adding an ammonium source and a fluorine source to a mixed solution containing a rare earth metal salt, an alkaline earth metal salt and a metal chelating agent, and preparing the composite luminescent material through a hydrothermal reaction; The metal chelating agent is a polycarboxylic acid compound, all the reaction raw materials are soluble substances, the polycarboxylic acid compound is at least one of sodium citrate or potassium citrate, and the ammonium source and fluoride source are a mixture of ammonium chloride and fluoride salt or at least one of ammonium fluoride.
2. The composite luminescent material according to claim 1, characterized in that: The particle size of the composite luminescent material is between 10nm and 20nm.
3. The composite luminescent material according to claim 1, characterized in that: The wavelength of the visible light is between 380nm and 650nm; and / or the peak value of the near-infrared light is between 950nm and 1050nm.
4. The composite luminescent material according to claim 1, characterized in that: The peak value of the near infrared light is 980 nm.
5. The composite luminescent material according to claim 1, characterized in that: The surface of the carbon dots contains at least one of a carboxyl group and an amino group.
6. The composite luminescent material according to claim 1, characterized in that: The alkaline earth metal element is selected from at least one of Ca, Sr and Ba.
7. The composite luminescent material according to claim 1, characterized in that: The molar ratio of the rare earth element to the total metal elements in the composite material is above 1:
100.
8. The composite luminescent material according to claim 1, characterized in that: The molar ratio of the rare earth element to the total metal elements in the composite material is greater than 1:
100.
9. The composite luminescent material according to claim 1, characterized in that: The molar ratio of the rare earth element to the total metal elements in the composite material is 1-5:
100.
10. The composite luminescent material according to claim 1, characterized in that: The molar ratio of the rare earth element to the alkaline earth metal element is 3:
100.
11. A method for preparing the composite luminescent material according to claim 1, characterized in that: The method comprises the following steps: adding an ammonium source and a fluorine source to a mixed solution containing a rare earth metal salt, an alkaline earth metal salt and a metal chelating agent, and preparing the composite luminescent material through a hydrothermal reaction; Wherein, the metal chelating agent is a polycarboxylic acid compound, and all reaction raw materials are soluble substances.
12. The preparation method according to claim 11, characterized in that: The temperature of the hydrothermal reaction is 150° C. to 200° C.; and / or the time of the hydrothermal reaction is 3 h to 8 h.
13. A light source, characterized in that: The light source comprises the composite luminescent material according to any one of claims 1 to 10.