Hydroxyapatite ceramic slurry for photocuring three-dimensional printing and preparation method thereof
By using the combination of silicon carbide whiskers and tertiary particle size modified hydroxyapatite in photocuring three-dimensional printing, the problem of insufficient strength and toughness of traditional bone stents is solved, and the preparation of high-strength and high-toughness bone stents is achieved. Suitable for the bearing parts of human bones.
Patent Information
- Application Number
- CN202310620817.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-05-29
AI Technical Summary
The bone stents prepared by traditional hydroxyapatite/liquid resin composites have low strength and poor toughness, making them difficult to apply to the load-bearing parts of human bones, and it is difficult to accurately control the shape and size of the inner holes.
Using silicon carbide whiskers and three-level particle size modified hydroxyapatite as components, through ultrasonic dispersion and stirring, combined with photoinitiator, ceramic slurry for photocuring three-dimensional printing is prepared to improve its structural strength and toughness.
The preparation of high structural strength and high toughness bone stents is achieved, with a fracture toughness of up to 3.5MPa·m1/2, a compressive strength of up to 90MPa, and a good slurry flowability, which is suitable for three-dimensional printing of complex shapes.
Smart Images

Figure CN116730654B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparing porous bone scaffolds by photocuring three-dimensional printing, and in particular to a hydroxyapatite ceramic slurry for photocuring three-dimensional printing and a preparation method thereof. Background Art
[0002] Currently, many people are suffering from bone defects due to various reasons such as traffic accidents, bone tumors and infections. Although the human skeleton can repair small bone defects by itself, there is still no effective treatment for large bone defects. However, with the rapid development of various scientific and technological advances, scientists have proposed a new treatment strategy - bone tissue engineering.
[0003] Bone tissue engineering uses porous bone scaffold structures to provide cells with space for life activities such as growth, proliferation and differentiation, while providing certain support functions for the human body. Geometric features such as pore shape, pore size and porosity significantly affect the elastic modulus and compressive strength of the bone scaffold, and also affect the proliferation rate and differentiation phenotype of bone cells, so it is very important to manufacture high-precision, structurally controllable porous bone scaffolds. In traditional bone scaffold manufacturing methods, the shape and size of the inner pores are difficult to accurately control, and light-curing three-dimensional printing technology can overcome the above defects. Hydroxyapatite is very similar to the inorganic components of natural bone, so it has good biocompatibility, osteoconductivity and osteoinductivity, and can be used as a raw material for printing materials. However, the bone scaffold structure prepared using hydroxyapatite / liquid resin composite materials as printing materials has low strength and poor toughness, and is more prone to cracks and brittle fractures, so it is difficult to apply to the load-bearing parts of human bones.
[0004] Therefore, it is of great significance to develop a ceramic slurry that can be used to prepare bone scaffolds with high structural strength and high toughness. Summary of the invention
[0005] The first object of the present invention is to provide a hydroxyapatite ceramic slurry for photocuring three-dimensional printing, which can prepare a bone scaffold with high structural strength and high toughness.
[0006] The second object of the present invention is to provide a method for preparing hydroxyapatite ceramic slurry for photocuring three-dimensional printing.
[0007] The present invention provides a hydroxyapatite ceramic slurry for photocuring three-dimensional printing, which comprises the following components in weight percentage: 2-6wt% silicon carbide whisker, 38-50wt% modified hydroxyapatite with a tertiary particle size, 43-59wt% premix and 1-2wt% photoinitiator; the premix comprises the following components in weight fraction: 58-64wt% deionized water, 24-31wt% ammonium acryloyl, 1-2wt% methylenebisacrylamide and 7-10.5wt% glycerol.
[0008] Preferably, the silicon carbide whisker has a diameter of 0.1-2.5 μm and a length of 10-30 μm. The silicon carbide whisker used in the present invention is a β-type cubic crystal system, colorless and transparent, with a refractive index of 2.65, which ensures the propagation of light during the photocuring process and reduces scattering.
[0009] Preferably, the premixed liquid comprises the following components in terms of weight fractions: 62 wt % of deionized water, 29 wt % of ammonium acrylamide, 1.5 wt % of methylene bisacrylamide and 7.5 wt % of glycerol.
[0010] Preferably, the modified hydroxyapatite of the three particle sizes comprises, by weight percentage: 65-76wt% of modified hydroxyapatite of 5-10μm particle size, 15-20wt% of modified hydroxyapatite of 100nm-1μm particle size and 8.9-15.7wt% of modified hydroxyapatite of 5-10nm particle size.
[0011] Preferably, the modification method of the modified hydroxyapatite is to dissolve ammonium polyacrylate in deionized water, add hydroxyapatite, and simultaneously disperse and stir by ultrasonication to obtain a suspension, filter the suspension, freeze-dry it, and sieve it to obtain surface-modified hydroxyapatite. The above modification method can make ammonium polyacrylate uniformly wrap hydroxyapatite, change the surface activity of hydroxyapatite, and further change the Zeta potential of the hydroxyapatite surface in the final slurry, and improve the stability and uniformity of the slurry through electrostatic steric effect and steric hindrance effect.
[0012] Preferably, in the modification method of modified hydroxyapatite, the mass ratio between the ammonium polyacrylate and deionized water is 1:1800.
[0013] Preferably, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone and / or methyl benzoylformate.
[0014] Preferably, the photoinitiator is methyl benzoylformate.
[0015] When the photoinitiator is 1-hydroxycyclohexyl phenyl ketone and methyl benzoylformate, the mass ratio of the two is 1:1.
[0016] The present invention also provides a method for preparing a hydroxyapatite ceramic slurry for photocuring three-dimensional printing, comprising the following steps:
[0017] (1) mixing water, ammonium acryloyl, methylenebisacrylamide and glycerol, stirring, heating and continuing stirring to obtain a premixed solution;
[0018] (2) adding the modified hydroxyapatite of the third-level particle size to the premixed liquid obtained in step (1), ultrasonically dispersing, and stirring to obtain a hydroxyapatite suspension of the third-level particle size; ammonium polyacrylate can modify the surface of hydroxyapatite and enhance the wettability of hydroxyapatite in the premixed liquid. The use of hydroxyapatite of the third-level particle size can better balance the contradiction between the fluidity of the slurry and the density of the printed product, thereby improving the fluidity of the slurry while ensuring the density of the three-dimensional printed product;
[0019] (3) adding silicon carbide whiskers to the suspension obtained in step (2), ultrasonically dispersing and stirring to obtain a silicon carbide whisker-reinforced tertiary particle size hydroxyapatite suspension;
[0020] (4) Adding a photoinitiator to the suspension obtained in step (3), stirring evenly, and obtaining a hydroxyapatite ceramic slurry for photocuring 3D printing.
[0021] Preferably, the specific steps of step (1) are: deionized water, ammonium acryloyl, methylene bisacrylamide and glycerol are mixed in proportion, stirred at a temperature of 25° C. at a rate of 200-400 rpm for 10-20 minutes, then the temperature is increased to 45° C., and stirred at a rate of 400-600 rpm for 10-15 minutes to obtain a premixed solution.
[0022] The hydroxyapatite ceramic slurry for photocuring 3D printing obtained by the present invention is used for photocuring 3D printing, and the photocuring parameters used are: ultraviolet laser power 1.2-2.8W, spot diameter 0.1-0.3mm, layer thickness 0.1-0.2mm, and scanning speed 1200-2300mm / s.
[0023] Beneficial effects:
[0024] The present invention uses silicon carbide whiskers as a toughening phase to improve the toughness and strength of light-cured hydroxyapatite. Compared with the untoughened state, the fracture toughness can reach 3.5MPa·m 1 / 2 , the compressive strength can reach 90MPa. By matching the three-level particle size modified hydroxyapatite, the slurry viscosity is guaranteed to be less than 7Pa·s, with good fluidity, which improves the applicability of light-curing 3D printing.
[0025] In the preparation method of the present invention, a premixed liquid is first prepared, modified hydroxyapatite with three-level particle sizes is added thereto, and then silicon carbide whiskers are added, which can effectively reduce whisker agglomeration and destruction. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 This is a rendering of the hydroxyapatite ceramic material obtained by photocuring three-dimensional printing of the product of Example 1 of the present invention. DETAILED DESCRIPTION
[0028] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0029] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] A hydroxyapatite ceramic slurry for photocuring three-dimensional printing comprises the following components in weight percentage: 2wt% silicon carbide whisker, 38wt% modified hydroxyapatite of tertiary particle size, 59wt% premix and 1wt% photoinitiator 1-hydroxycyclohexyl phenyl ketone; the premix comprises the following components in weight fraction: 64wt% deionized water, 24wt% ammonium acrylamide, 1.5wt% methylenebisacrylamide and 10.5wt% glycerol. The diameter of the silicon carbide whisker is 0.1-2.5μm and the length is 10-30μm. The silicon carbide whisker used in the present invention is a β-type cubic system, colorless and transparent, with a refractive index of 2.65, which ensures the propagation of light during the photocuring process and reduces scattering.
[0033] The modification method of modified hydroxyapatite is as follows: dissolving ammonium polyacrylate in deionized water to obtain an ammonium polyacrylate solution, wherein the mass ratio of ammonium polyacrylate to deionized water is 1:1800, adding hydroxyapatite with a particle size of 5-10 μm, wherein the volume ratio of hydroxyapatite to the ammonium polyacrylate solution is 1:2, and ultrasonic dispersion is performed by an ultrasonic disperser, and stirring is performed at a rate of 1200 rpm for 22 minutes to obtain a hydroxyapatite powder suspension with a particle size of 5-10 μm, and then the suspension is filtered, freeze-dried at -20°C, and sieved to obtain surface-modified hydroxyapatite with a particle size of 5-10 μm; the above modification method can make ammonium polyacrylate uniformly wrap hydroxyapatite, change the surface activity of hydroxyapatite, enhance the wettability of hydroxyapatite in the premixed solution, and further change the Zeta potential of the hydroxyapatite surface in the final slurry, thereby improving the slurry stability and uniformity through electrostatic steric effect and spatial steric effect;
[0034] The surface of hydroxyapatite with a particle size of 100 nm-1 μm and hydroxyapatite with a particle size of 5-10 nm was modified according to the above method.
[0035] A method for preparing a hydroxyapatite ceramic slurry for photocuring three-dimensional printing comprises the following steps:
[0036] (1) mixing 64 wt % of deionized water, 24 wt % of ammonium acryloyl, 1.5 wt % of methylenebisacrylamide and 10.5 wt % of glycerol in a weight ratio, stirring at 300 rpm for 15 minutes at 25° C., then raising the temperature to 45° C. and stirring at 500 rpm for 13 minutes to obtain a premixed solution;
[0037] (2) preparing modified hydroxyapatite with a tertiary particle size according to the weight fractions of 70wt% of modified hydroxyapatite with a particle size of 5-10μm, 18wt% of modified hydroxyapatite with a particle size of 100nm-1μm and 12wt% of modified hydroxyapatite with a particle size of 5-10nm, adding the mixture to the premixed solution obtained in step (1), performing ultrasonic dispersion, and stirring to obtain a hydroxyapatite suspension with a tertiary particle size; the use of modified hydroxyapatite with a tertiary particle size can better balance the contradiction between the fluidity of the slurry and the density of the printed product, thereby improving the fluidity of the slurry while ensuring the density of the three-dimensional printed product;
[0038] (3) adding silicon carbide whiskers to the suspension obtained in step (2), ultrasonically dispersing and stirring to obtain a silicon carbide whisker-reinforced tertiary particle size hydroxyapatite suspension;
[0039] (4) Adding a photoinitiator, 1-hydroxycyclohexyl phenyl ketone, to the suspension obtained in step (3), stirring the mixture evenly, and obtaining a hydroxyapatite ceramic slurry for photocuring 3D printing.
[0040] The hydroxyapatite ceramic slurry for photocuring 3D printing obtained in Example 1 is used for photocuring 3D printing to obtain hydroxyapatite ceramic material. The effect diagram is as follows: Figure 1 The light curing parameters used are: UV laser power 2.2W, spot diameter 0.2mm, layer thickness 0.15mm, scanning speed 1800mm / s.
[0041] Example 2
[0042] A hydroxyapatite ceramic slurry for photocuring three-dimensional printing comprises the following components by weight percentage: 6wt% silicon carbide whisker, 50wt% modified hydroxyapatite with a three-level particle size, 43wt% premixed liquid and 1wt% photoinitiator methyl benzoylformate; the premixed liquid comprises the following components by weight fraction: 58wt% deionized water, 29.3wt% ammonium acryloyl, 2.5wt% methylenebisacrylamide and 10.2wt% glycerol. The diameter of the silicon carbide whisker is 0.1-2.5μm and the length is 10-30μm. The silicon carbide whisker used in the present invention is a β-type cubic system, colorless and transparent, with a refractive index of 2.65, so as to ensure the propagation of light during the photocuring process and reduce scattering.
[0043] The modification method of modified hydroxyapatite is as follows: dissolving ammonium polyacrylate in deionized water to obtain an ammonium polyacrylate solution, wherein the mass ratio of ammonium polyacrylate to deionized water is 1:1600, adding hydroxyapatite with a particle size of 5-10 μm, and simultaneously performing ultrasonic dispersion using an ultrasonic disperser, stirring at a rate of 1000 rpm for 30 minutes, and the volume ratio of hydroxyapatite to the ammonium polyacrylate solution is 1:3, to obtain a hydroxyapatite powder suspension with a particle size of 5-10 μm, and then filtering the suspension, freeze-drying at -20°C, and sieving to obtain surface-modified hydroxyapatite with a particle size of 5-10 μm; the above modification method can make ammonium polyacrylate uniformly wrap hydroxyapatite, change the surface activity of hydroxyapatite, enhance the wettability of hydroxyapatite in the premixed solution, and further change the Zeta potential of the hydroxyapatite surface in the final slurry, thereby improving the slurry stability and uniformity through electrostatic steric effect and spatial steric effect;
[0044] The surface of hydroxyapatite with a particle size of 100 nm-1 μm and hydroxyapatite with a particle size of 5-10 nm was modified according to the above method.
[0045] A method for preparing a hydroxyapatite ceramic slurry for photocuring three-dimensional printing comprises the following steps:
[0046] (1) mixing 62 wt % of deionized water, 29 wt % of ammonium acryloyl, 1.5 wt % of methylenebisacrylamide and 7.5 wt % of glycerol in a weight ratio, stirring at 200-400 rpm for 10-20 minutes at 25° C., then raising the temperature to 45° C., stirring at 400-600 rpm for 10-15 minutes to obtain a premixed solution;
[0047] (2) adding modified hydroxyapatite with three-level particle sizes according to the weight fractions of 65wt% of modified hydroxyapatite with a particle size of 5-10μm, 20wt% of modified hydroxyapatite with a particle size of 100nm-1μm and 15wt% of modified hydroxyapatite with a particle size of 5-10nm to the premixed solution obtained in step (1), ultrasonically dispersing, and stirring to obtain a hydroxyapatite suspension with three-level particle sizes; the use of modified hydroxyapatite with three-level particle sizes can better balance the contradiction between the fluidity of the slurry and the density of the printed product, thereby improving the fluidity of the slurry while ensuring the density of the three-dimensional printed product;
[0048] (3) adding silicon carbide whiskers to the suspension obtained in step (2), ultrasonically dispersing and stirring to obtain a silicon carbide whisker-reinforced tertiary particle size hydroxyapatite suspension;
[0049] (4) Adding a photoinitiator, methyl benzoylformate, to the suspension obtained in step (3), stirring the mixture evenly, and obtaining a hydroxyapatite ceramic slurry for photocuring 3D printing.
[0050] The hydroxyapatite ceramic slurry for photocuring 3D printing obtained in Example 2 was used for photocuring 3D printing to obtain hydroxyapatite ceramic material. The photocuring parameters used were: UV laser power 1.2 W, spot diameter 0.3 mm, layer thickness 0.2 mm, and scanning speed 1200 mm / s.
[0051] Example 3
[0052] A hydroxyapatite ceramic slurry for photocuring three-dimensional printing comprises the following components by weight percentage: 3wt% silicon carbide whisker, 40wt% modified hydroxyapatite of tertiary particle size, 55wt% premix and 2wt% photoinitiator, wherein the photoinitiator is composed of 1-hydroxycyclohexyl phenyl ketone and methyl benzoylformate in a mass ratio of 1:1; the premix comprises the following components by weight fraction: 58wt% deionized water, 31wt% ammonium acrylamide, 2wt% methylenebisacrylamide and 9wt% glycerol. The diameter of the silicon carbide whisker is 0.1-2.5μm and the length is 10-30μm. The silicon carbide whisker used in the present invention is a β-type cubic system, colorless and transparent, with a refractive index of 2.65, so as to ensure the propagation of light during the photocuring process and reduce scattering.
[0053] The modification method of modified hydroxyapatite is as follows: dissolving ammonium polyacrylate in deionized water to obtain an ammonium polyacrylate solution, wherein the mass ratio of ammonium polyacrylate to deionized water is 1:1700, adding hydroxyapatite with a particle size of 5-10 μm, wherein the volume ratio of hydroxyapatite to the ammonium polyacrylate solution is 1:2, and ultrasonic dispersion is performed by an ultrasonic disperser, and stirring is performed at a rate of 1500 rpm for 15 minutes to obtain a hydroxyapatite powder suspension with a particle size of 5-10 μm, and then the suspension is filtered, freeze-dried at -20°C, and sieved to obtain surface-modified hydroxyapatite with a particle size of 5-10 μm; the above modification method can make ammonium polyacrylate uniformly wrap hydroxyapatite, change the surface activity of hydroxyapatite, enhance the wettability of hydroxyapatite in the premixed solution, and further change the Zeta potential of the hydroxyapatite surface in the final slurry, thereby improving the slurry stability and uniformity through electrostatic steric effect and spatial steric effect;
[0054] The surface of hydroxyapatite with a particle size of 100 nm-1 μm and hydroxyapatite with a particle size of 5-10 nm was modified according to the above method.
[0055] The present invention also provides a method for preparing a hydroxyapatite ceramic slurry for photocuring three-dimensional printing, comprising the following steps:
[0056] (1) mixing 58 wt % of deionized water, 31 wt % of ammonium acryloyl, 2 wt % of methylenebisacrylamide and 9 wt % of glycerol in a weight ratio, stirring at 200-400 rpm for 10-20 minutes at 25° C., then raising the temperature to 45° C., stirring at 400-600 rpm for 10-15 minutes to obtain a premixed solution;
[0057] (2) adding modified hydroxyapatite with three-level particle sizes according to the weight fractions of 76wt% of modified hydroxyapatite with a particle size of 5-10μm, 15wt% of modified hydroxyapatite with a particle size of 100nm-1μm and 9wt% of modified hydroxyapatite with a particle size of 5-10nm to the premixed solution obtained in step (1), ultrasonically dispersing, and stirring to obtain a hydroxyapatite suspension with three-level particle sizes; the use of modified hydroxyapatite with three-level particle sizes can better balance the contradiction between the fluidity of the slurry and the density of the printed product, thereby improving the fluidity of the slurry while ensuring the density of the three-dimensional printed product;
[0058] (3) adding silicon carbide whiskers to the suspension obtained in step (2), ultrasonically dispersing and stirring to obtain a silicon carbide whisker-reinforced tertiary particle size hydroxyapatite suspension;
[0059] (4) Add the mixed photoinitiator benzene 1-hydroxycyclohexyl phenyl ketone and methyl benzoylformate to the suspension obtained in step (3), stir evenly, and obtain a hydroxyapatite ceramic slurry for photocuring three-dimensional printing.
[0060] The hydroxyapatite ceramic slurry for photocuring 3D printing obtained in Example 3 was used for photocuring 3D printing to obtain hydroxyapatite ceramic material. The photocuring parameters used were: UV laser power 2.8 W, spot diameter 0.1 mm, layer thickness 0.1 mm, and scanning speed 2300 mm / s.
[0061] Comparative Example 1
[0062] A hydroxyapatite ceramic slurry for photocuring three-dimensional printing comprises the following components in weight percentage: 55wt% of hydroxyapatite, 43wt% of premixed liquid and 2wt% of photoinitiator 1-hydroxycyclohexyl phenyl ketone; the premixed liquid comprises the following components in weight fraction: 58wt% of deionized water, 29.3wt% of ammonium acrylamide, 2.5wt% of methylenebisacrylamide and 10.2wt% of glycerol.
[0063] A method for preparing a hydroxyapatite ceramic slurry for photocuring three-dimensional printing comprises the following steps:
[0064] (1) mixing 58 wt % of deionized water, 29.3 wt % of ammonium acryloyl, 2.5 wt % of methylenebisacrylamide and 10.2 wt % of glycerol in a weight ratio, stirring at 200-400 rpm for 10-20 minutes at 25° C., then raising the temperature to 45° C., stirring at 400-600 rpm for 10-15 minutes to obtain a premixed solution;
[0065] (2) adding 20 wt % hydroxyapatite to the premixed solution obtained in step (1), dispersing by ultrasonication, and stirring to obtain a hydroxyapatite suspension;
[0066] (3) Add 2 wt % of a photoinitiator, 1-hydroxycyclohexyl phenyl ketone, to the suspension obtained in step (2), and stir evenly to obtain a hydroxyapatite ceramic slurry for photocuring 3D printing.
[0067] The hydroxyapatite ceramic slurry for photocuring 3D printing obtained in Comparative Example 1 was used for photocuring 3D printing to obtain hydroxyapatite ceramic material. The photocuring parameters used were: UV laser power 1.2 W, spot diameter 0.3 mm, layer thickness 0.2 mm, and scanning speed 1200 mm / s.
[0068] Performance Test:
[0069] The hydroxyapatite ceramic slurry for photocuring 3D printing obtained by using Examples 1-3 and Comparative Example 1 was subjected to a fluidity test, and the slurry obtained by Examples 1-3 and Comparative Example 1 was subjected to photocuring 3D printing to obtain a hydroxyapatite ceramic material for a mechanical property test to detect its fracture toughness, compressive strength and density. The test results are shown in Table 1.
[0070] Table 1
[0071]
[0072] As shown in Table 1, the final photocured products of Examples 1-3 have a fracture toughness of up to 3.5 MPa·m compared with Comparative Example 1 before toughening. 1 / 2 (about 150% increase), and the compressive strength can reach 90MPa (about 170% increase).
[0073] The higher the fluidity of the slurry in Examples 1-3, the lower the density of the material obtained by photocuring printing. The density of Example 2 is 2.7 g / cm 3 , which is higher than that of the product in comparative example 1. The density of the photocured printed material is 2.6 g / cm 3 , the fluidity of Example 2 is also better than that of Comparative Example 1. By matching the three-level particle size modified hydroxyapatite, the slurry viscosity is ensured to be less than 7Pa·s, and the slurry has good fluidity. The fracture toughness and compressive strength of Example 2 are the best, which shows that the comprehensive performance of Example 2 is better than that of Comparative Example 1. The hydroxyapatite ceramic slurry for photocuring 3D printing provided by the present invention improves the applicability of photocuring 3D printing, can give full play to the advantages of photocuring 3D printing, and can manufacture complex shapes.
[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A hydroxyapatite ceramic slurry for photocuring 3D printing, characterized in that: The invention comprises the following components according to weight percentage: 2-6wt% silicon carbide whisker, wherein the silicon carbide whisker has a diameter of 0.1-2.5μm and a length of 10-30μm; 38-50wt% modified hydroxyapatite of tertiary particle size, 43-59wt% premix and 1-2wt% photoinitiator; the premix comprises the following components according to weight fraction: 58-64wt% deionized water, 24-31wt% acrylamide, 1-2wt% methylenebisacrylamide and 7-10.5wt% glycerol, and the sum of the weight fractions of the components is 100%; The modified hydroxyapatite of the three-level particle size is composed of the following components in weight percentage: 65-76wt% of modified hydroxyapatite with a particle size of 5-10μm, 15-20wt% of modified hydroxyapatite with a particle size of 100nm-1μm, and 8.0-15.7wt% of modified hydroxyapatite with a particle size of 5-10nm; The modification method of the modified hydroxyapatite is to dissolve ammonium polyacrylate in deionized water to obtain an ammonium polyacrylate solution, add hydroxyapatite, and simultaneously perform ultrasonic dispersion and stirring to obtain a suspension, filter the suspension, freeze-dry it, and sieve it to obtain surface-modified hydroxyapatite; the volume ratio of the hydroxyapatite to the ammonium polyacrylate solution is 1:3-1:2, and the mass ratio between the ammonium polyacrylate and the deionized water in the modification method of the modified hydroxyapatite is 1:1800-1:1600.
2. The hydroxyapatite ceramic slurry for photocuring 3D printing according to claim 1, characterized in that: The premixed liquid includes the following components by weight: 62 wt % of deionized water, 29 wt % of acrylamide, 1.5 wt % of methylene bisacrylamide and 7.5 wt % of glycerol.
3. The hydroxyapatite ceramic slurry for photocuring 3D printing according to claim 1, characterized in that: The photoinitiator is 1-hydroxycyclohexyl phenyl ketone and / or methyl benzoylformate.
4. The hydroxyapatite ceramic slurry for photocuring 3D printing according to claim 3, characterized in that: The photoinitiator is methyl benzoylformate.
5. The method for preparing the hydroxyapatite ceramic slurry for photocuring 3D printing according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Mix deionized water, acrylamide, methylenebisacrylamide and glycerol, stir, heat and continue stirring to obtain a premixed solution; (2) adding the modified hydroxyapatite of the third-grade particle size into the premixed solution obtained in step (1), dispersing by ultrasonication, and stirring to obtain a hydroxyapatite suspension of the third-grade particle size; (3) adding silicon carbide whiskers to the suspension obtained in step (2), dispersing by ultrasonication and stirring evenly to obtain a silicon carbide whisker-toughened hydroxyapatite suspension of three-grade particle size; (4) Adding a photoinitiator to the suspension obtained in step (3), stirring evenly, and obtaining a hydroxyapatite ceramic slurry for photocuring 3D printing.
6. The preparation method according to claim 5, characterized in that: The specific steps of step (1) are: deionized water, acrylamide, methylenebisacrylamide and glycerol are mixed in proportion, stirred at a temperature of 25° C. at a rate of 200-400 rpm for 10-20 minutes, then the temperature is increased to 45° C., and stirred at a rate of 400-600 rpm for 10-15 minutes to obtain a premixed solution.