A method and application of vertical connection between anode steel claw and anode aluminum guide rod of electrolytic cell

Through self-propagation casting method and water-cooled tank cooling technology, the stable connection between the anode steel claw and the aluminum guide rod is achieved, solving the problems of complex connection, high cost and large pressure drop in the existing technology, and significantly reducing the energy of electrolytic aluminum production Consumption and pressure drop.

CN116752196BActive Publication Date: 2024-11-19NINGXIA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310754867.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-25
Publication Date
2024-11-19
Estimated Expiration
2043-06-25

AI Technical Summary

Technical Problem

The existing connection method of electrolytic aluminum anode steel claws and aluminum guide rods has problems such as complex process, high cost, high voltage drop in the connection area and large energy consumption.

Method used

The anode steel claws and aluminum guide rods are connected vertically by self-propagation melting and casting method, and the welding gap is filled with the casting mold and self-propagation powder, and combined with water-cooling tank cooling to form a Fe-Al intermetallic compound layer, simplifying the process flow and reducing the pressure drop .

Benefits of technology

The stable and reliable connection between the anode steel claws and the aluminum guide rod is achieved, which significantly reduces the pressure drop in the connection area, simplifies the process flow, and reduces production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116752196B_ABST
    Figure CN116752196B_ABST
Patent Text Reader

Abstract

The present invention provides a method for vertical connection of an anode steel claw and an anode aluminum guide rod of an electrolytic cell, comprising the following steps: roughening the surface of the steel claw boss and placing the anode steel claw vertically; vertically suspending the aluminum guide rod above the steel claw boss so that a welding gap is left between the connection end and the steel claw boss; setting a melting and casting mold, filling the mold connection gap, and preheating the melting and casting mold and the steel claw boss; igniting the self-propagating powder in the melting and casting mold so that the molten metal flows into and fills the welding gap; cooling the steel claw, removing the mold, and performing a shaping treatment on the connection part. The present invention also provides an anode conductive component of an electrolytic aluminum process based on the above method. The present invention directly connects the anode guide rod to the steel claw, has a simple process, does not require large equipment, avoids the use of aluminum-steel explosion blocks, reduces the number of welding passes and joints, improves efficiency and ensures welding quality, has a low pressure drop in the connection area, strong bonding strength, and high interface quality, ensuring the use effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum smelting, and specifically relates to a method for vertically connecting an anode steel claw and an anode aluminum guide rod of an electrolytic cell, and also relates to an anode conductive component of an aluminum electrolytic process based on the connection method. Background Art

[0002] In recent years, my country's electrolytic aluminum industry has developed rapidly, and its electrolytic aluminum production ranks first in the world. Electrolytic aluminum anode components often need to withstand loads, high currents and high temperature environments during operation, so the performance requirements of anode components are extremely high. At present, in electrolytic aluminum enterprises, the anode structure of the electrolytic cell usually places the anode aluminum guide rod and the anode steel claw horizontally, and then uses the aluminum-steel explosion block as the transition structure, and connects them by aluminum-aluminum and steel-steel welding respectively. However, this connection method has the following problems: (1) The guide rod and the steel claw are connected by the explosion block, and there are three contact pressure drop joint surfaces: aluminum-aluminum weld, steel-steel weld and the steel-aluminum joint of the explosion block, which leads to high resistance and high energy consumption of the anode device during use. (2) The traditional method uses an explosion block to connect the guide rod and the steel claw, which requires at least two weldings. Due to the large cross-sectional dimensions of the guide rod and the steel claw, the welding cost is high. (3) The traditional welding method requires the guide rod and the steel claw to be placed horizontally, and a large groove is opened at the welding position, which is complicated and inefficient.

[0003] In order to solve the above problems, researchers have provided a variety of different improvement schemes for the connection between the anode steel claw and the anode aluminum guide rod. For example, the anode conductive device for aluminum electrolysis described in patent CN216141636U is composed of an aluminum guide rod, an anode steel claw, and a steel-aluminum connector. The conductive area is limited by welding the aluminum rod and the guide rod side. If the conductive area of ​​the device is to be increased, the number of steel-aluminum connectors must be increased; the steel-aluminum connector uses a steel sleeve to increase the strength, which makes the overall weight and size of the device too large, the structure is complex, and the production cost is high, which increases the difficulty of device maintenance and replacement. Patent CN109518229A describes a method of connecting the anode guide rod and the steel claw by friction welding. This method requires the consumption of aluminum guide rods and uses large friction welding equipment, which is too expensive and difficult to promote on a large scale. Patent CN109338412A describes an anode steel claw connected by welding and support bolts and an assembly method thereof, which improves strength by adding bolt connections between the aluminum guide rod and the steel claw, but the process is complicated and the processing of through holes on the guide rod can easily lead to uneven distribution of the anode current, and the high-temperature corrosion of the bolts increases the maintenance cost of the equipment; Patent CN110257860A describes a composite-formed anode conductive device and a manufacturing method thereof, which welds the aluminum guide rod and the steel claw by adding auxiliary steel plates, but this method chooses vertical welding. If the welding quality is to be guaranteed, a large-sized groove needs to be made at the interface between the auxiliary plate and the steel claw, which invisibly increases the construction difficulty, increases the cost, and reduces the production efficiency.

[0004] Based on this, it is urgent to develop a new connection method between the anode steel claw and the anode aluminum guide rod of the electrolytic cell, so as to effectively solve the problems existing in the connection between the existing anode steel claw and the aluminum guide rod, such as complex process, high production cost, high voltage drop in the connection area, and high energy consumption. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for vertically connecting an anode steel claw and an anode aluminum guide rod of an electrolytic cell, which has simple and easy operation procedures, high connection stability, and significantly reduces the voltage drop in the connection area.

[0006] A second object of the present invention is to provide an anode conductive component for an electrolytic aluminum process having high connection stability and low voltage drop in the connection area.

[0007] The technical solution adopted by the present invention to achieve one of the purposes is: to provide a method for vertically connecting an anode steel claw and an anode aluminum guide rod of an electrolytic cell, comprising the following steps:

[0008] S1. Roughening the surface of the steel claw boss of the anode steel claw, and then placing the anode steel claw vertically;

[0009] S2, pre-treating the connecting end of the aluminum guide rod, and vertically hanging the aluminum guide rod above the steel claw boss, so that a welding gap is left between the connecting end and the steel claw boss;

[0010] S3, surrounding the casting mold around the connection end, the welding gap and the outer side of the steel claw boss, fixing the casting mold and filling the connection gap, placing self-propagating casting powder, and preheating the casting mold and the steel claw boss;

[0011] S4, when the steel claw boss is preheated to a specified temperature, igniting the self-propagating casting powder in the casting mold, so that the molten metal flows into and fills the welding gap;

[0012] S5. Cool the steel claw, remove the mold, and perform shaping treatment on the connection part, thus completing the vertical connection of the anode steel claw and the anodized aluminum guide rod.

[0013] The general idea of ​​the present invention is as follows: the present invention provides a method for vertically connecting an anode aluminum guide rod and an anode steel claw. Under the premise that the steel claw and the aluminum guide rod are placed vertically and a welding gap is left, the molten metal liquid after the self-propagating powder reaction is filled into the welding gap between the connecting end of the aluminum guide rod and the steel claw boss through the auxiliary effect of the casting mold; finally, by directly cooling the steel claw and indirectly cooling the casting joint, it is ensured that a sufficient Fe-Al intermetallic compound layer can be generated between the aluminum guide rod and the anode steel claw during the connection process, providing metallurgical bonding to ensure bonding strength, and controlling the growth time of the brittle and hard intermetallic compound layer to avoid excessive thickness and reduce the connection quality. The above method can effectively solve the problems of complex procedures, high pressure drop, easy separation of the steel claw and the aluminum guide rod, and uneven pressure drop distribution caused by differences in the composition of the welding area in the traditional explosive block connection method, realize a stable and reliable connection between the anode steel claw and the anode aluminum guide rod, and can significantly reduce the pressure drop in the connection area.

[0014] In step S1, the anode steel claw includes a steel claw beam and a steel claw foot. The material of the steel claw beam and the steel claw foot is preferably Q235 or ordinary cast steel, and the casting method is preferably sand casting or lost foam casting. Further, the steel claw boss is arranged on the top of the steel claw beam and is made by an integrated processing and molding method with the steel claw beam.

[0015] Furthermore, the steel claw boss is provided with a protrusion and / or a recessed structure on one side facing the connection end. Preferably, a T-shaped protrusion structure with a height of 140 to 160 mm and a length of 180 to 200 mm is welded on the side of the steel claw boss facing the connection end of the aluminum guide rod and / or a plurality of holes with a depth of 40 to 60 mm and a diameter of 20 to 25 mm are distributed. Such a structural design helps to improve the bonding strength between the steel claw and the connection part of the aluminum guide rod.

[0016] Preferably, in step S1, the roughening treatment of the surface of the steel claw boss can be performed by sandblasting or grinding wheel grinding.

[0017] Furthermore, in step S2, pre-treating the connection end of the aluminum guide rod includes: degreasing and descaling the connection end.

[0018] Furthermore, in step S2, the height of the welding gap is 30 to 40 cm. In the present invention, by controlling the distance of the welding gap, the speed at which the metal solution generated by the self-propagating reaction fills the space to be connected can be controlled, and the cooling start time can be further determined, thereby controlling the thickness of the intermetallic compound layer at the connection interface between the aluminum guide rod and the steel claw boss.

[0019] Furthermore, in step S3, the self-propagating melting casting mold includes: a gate mold, a riser mold, a front plugging mold and a rear plugging mold. Among them, the gate mold and the riser mold are placed in opposition, the front plugging mold and the rear plugging mold are respectively located on both sides of the gate mold and the riser mold, and the four molds are arranged in a surrounding manner on the outside of the parts to be connected (connecting ends, welding gaps and steel claw bosses). In the gate mold of the melting casting mold, a self-propagating crucible is placed, the bottom of the self-propagating crucible is opened and covered with a metal sheet (a sheet made of aluminum or aluminum alloy with a thickness of 3 to 5 mm and a diameter of 12 to 15 mm), and the self-propagating melting casting powder is contained in the self-propagating crucible. Furthermore, refractory clay is used to fix each mold, and refractory clay is used to fill the gaps between each mold and the connecting end, each mold and the steel claw boss, and each mold.

[0020] Preferably, in step S4, the designated temperature for preheating the steel claw boss is 650-800°C; more preferably, the designated temperature for preheating the steel claw boss is 700-750°C.

[0021] Furthermore, in step S4, the invention adopts a self-propagating method to connect the anode guide rod and the anode steel claw, and designs a special self-propagating casting material formula, which has stable reaction, safety and reliability, short processing time and low raw material price. On the one hand, sulfate acts as an oxidant and oxide to coordinate, so that the whole reaction process is stable and not too violent; on the other hand, it is used as a slag-forming agent. Lanthanide metal oxides can both serve as slag-forming agents and enhance the performance of molten-cast joints. The addition of slag-forming agents ensures the separation of slag and liquid during the connection process, thereby obtaining a high-quality interface.

[0022] In some preferred embodiments, the components of the self-propagating casting powder include, by mass fraction, 20% to 23% iron oxide, 4% to 6% copper oxide, 1% to 1.5% manganese oxide, 8% to 9% tin dioxide, 9% to 11% calcium sulfate, 4% to 6% magnesium sulfate, and 3% to 5% barium sulfate; the minimum mass percentage of the foregoing materials is not less than 50% to ensure that there is sufficient oxidant in the self-propagating system to provide reliable heat output; it also includes: 2.5% to 4% calcium fluoride, 0.2% to 0.25% lanthanide oxide, 4% silicon powder, 22% to 24% 300 mesh aluminum powder, and the rest is 100 mesh aluminum powder.

[0023] Furthermore, in step S4, during the process of filling the welding gap with molten metal, the filling condition of the molten metal is observed through the riser of the riser mold of the casting mold. After the riser is observed to be filled with the molten metal, the next step of cooling the steel claw is performed.

[0024] Furthermore, in step S5, the cooling of the steel claw is carried out by water cooling. In the present invention, the method of indirect cooling of the cast joint by self-propagating casting combined with flushing the anode steel claw with a water cooling tank not only ensures that a sufficient Fe-Al intermetallic compound layer can be generated between the aluminum guide rod and the anode steel claw during the connection process to provide metallurgical bonding to ensure bonding strength, but also controls the growth time of the brittle and hard intermetallic compound layer to avoid excessive thickness and reduction of the connection quality.

[0025] Specifically, the following method can be used: in step S1, first vertically place the anode steel claw in a water-free water cooling tank, and then perform subsequent operation steps; then in step S5, directly fill the water cooling tank with water to achieve rapid cooling of the steel claw. Preferably, the maximum water filling height in step S5 is located 10 to 15 cm below the upper plane of the steel claw crossbeam, which helps to control the cooling speed of the connection joint, prevent the water level from being too high, the cooling water from boiling and soaking on the joint, and prevent stress cracks caused by too fast cooling speed; it also avoids too low cooling water level, slow cooling rate of the joint, and too thick growth of the intermetallic compound layer.

[0026] Furthermore, in step S5, the shaping process includes cutting off the metal of the gate and the riser.

[0027] The technical solution adopted by the present invention to achieve the second purpose is: to provide an anode conductive component for an electrolytic aluminum process, including an anode aluminum guide rod and an anode steel claw, and the anode aluminum guide rod and the anode steel claw are connected using the method described in one of the purposes of the present invention.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The method for vertically connecting the anode steel claw and the anode aluminum guide rod of the electrolytic cell provided by the present invention adopts a method of directly connecting the anode guide rod and the steel claw, avoids the use of aluminum-steel explosion blocks as transition materials, reduces the number of welding passes and joints, and reduces the possibility of failure of the anode structure due to insufficient welding quality.

[0030] (2) The method for vertically connecting the anode steel claw and the anode aluminum guide rod of the electrolytic cell provided by the present invention adopts a self-propagating method to connect the anode guide rod and the anode steel claw. The self-propagating system has stable reaction, is safe and reliable, has a short processing time, and has low raw material prices. The coordination of sulfate and oxide in the self-propagating system makes the entire reaction process stable and not too intense. The addition of slag-forming agent ensures the separation of slag and liquid during the connection process, and a high-quality interface can be obtained.

[0031] (3) The method for vertically connecting the anode steel claw and the anode aluminum guide rod of the electrolytic cell provided by the present invention adopts a vertical connection method, which reduces the production of large welding grooves in the traditional welding of large-section anode parts, simplifies the process flow, and the entire connection process is simple, the tools are simple, and no other large equipment is required.

[0032] (4) The method for vertically connecting the anode steel claw and the anode aluminum guide rod of the electrolytic cell provided by the present invention adopts a method of directly cooling the steel claw after the self-propagating melting and casting connection, and indirectly cooling the melting and casting joint, which not only ensures that a sufficient Fe-Al intermetallic compound layer can be generated between the aluminum guide rod and the anode steel claw during the connection process to provide metallurgical bonding to ensure bonding strength, but also controls the growth time of the brittle and hard intermetallic compound layer to avoid excessive thickness and reduction of the connection quality.

[0033] (5) Compared with the traditional explosion block connection method, the anode conductive component of the electrolytic aluminum process manufactured by the method of vertically connecting the anode steel claw and the anode aluminum guide rod provided by the present invention has a significantly lower average pressure drop and good use effect, which can reduce the energy consumption and production cost of electrolytic aluminum production and is easy to promote and apply. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a flow chart of a method for vertically connecting a steel claw and an aluminum guide rod provided by an embodiment of the present invention;

[0035] Figure 2 It is a three-dimensional schematic diagram of the vertical connection between the steel claw and the aluminum guide rod provided by an embodiment of the present invention;

[0036] Figure 3 is a front view of the vertical connection between the steel claw and the aluminum guide rod provided in Example 1 of the present invention;

[0037] Figure 4 is a top view of the vertical connection between the steel claw and the aluminum guide rod provided in Example 1 of the present invention;

[0038] Figure 5 It is a schematic diagram of the structure of the vertical connection part between the steel claw and the aluminum guide rod provided in Example 2 of the present invention;

[0039] Figure 6 1 is a schematic diagram of the structure of the vertical connection part between the steel claw and the aluminum guide rod provided in Example 3 of the present invention;

[0040] In the figure: 1-1. Steel claw beam; 1-2. Steel claw foot; 1-3. Steel claw boss; 2. Aluminum guide rod; 3-1. Gate mold; 3-2. Riser mold; 3-3. Front plugging mold; 3-4. Rear plugging mold; 4-1. Self-propagating molten casting crucible; 4-2. Self-propagating molten casting material; 5. Water cooling tank; A. Steel claw boss plane; B. Outer convex surface of steel claw boss; C. Inner concave surface of steel claw boss. DETAILED DESCRIPTION

[0041] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0043] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0044] The composition (wt.%) of the self-propagating casting powder used in Examples 1-3 of the present invention is shown in Table 1 below.

[0045] Table 1

[0046]

[0047]

[0048] In the above table, the lanthanide oxides include lanthanum oxide, cerium oxide and a mixture of lanthanum oxide and cerium oxide.

[0049] Example 1

[0050] This embodiment provides a method for vertically connecting an anode steel claw and an anode aluminum guide rod of an electrolytic cell. The overall structure of the vertical connection between the steel claw and the aluminum guide rod is as follows: Figure 2 As shown, the connection method includes the following steps (such as Figure 1 ):

[0051] (1) Steel claw casting and welding: Use the lost foam casting method to cast the Q235 anode steel claw beam and steel claw foot, and weld the steel claw to the beam.

[0052] (2) Surface treatment of the steel claw boss: Use a grinding wheel to roughen the surface of the steel claw boss (such as Figure 3 and Figure 4 ).

[0053] (3) Docking and positioning of self-propagating casting parts: Degrease and descaling the connecting end of the aluminum guide rod, place the steel claw in a water-free water cooling tank, with the water level 10 cm below the upper plane of the steel claw beam. Hoist the guide rod and align it with the connecting end of the steel claw boss, with a distance of 30 cm between the two welding end faces.

[0054] (4) Preparation for self-propagating melting and casting: Place the self-propagating melting and casting mold around the connection between the aluminum guide rod and the steel claw boss, and ensure that the gate mold and the riser mold are placed in alignment. Use refractory clay to fix the mold and fill the gap between the molds. Open a hole at the bottom of the self-propagating melting and casting crucible and cover it with a 15mm diameter and 5mm thick pure aluminum sheet. Prepare the self-propagating melting and casting raw material powder, which can be: 20% iron oxide, 4% copper oxide, 1.5% manganese oxide, 8% tin dioxide, 9% calcium sulfate, 5% magnesium sulfate, 3% barium sulfate, 3% calcium fluoride, 0.25% lanthanide oxide, 4% silicon powder, 22% 300 mesh aluminum powder, and the rest is 100 mesh aluminum powder. Mix them evenly and place them in the self-propagating melting and casting crucible. Preheat the self-propagating melting and casting mold and the steel claw boss.

[0055] (5) Self-propagating casting: After the steel claw boss is preheated to 750°C, a self-propagating casting crucible is placed, the self-propagating casting powder is ignited, a self-propagating reaction occurs, and the molten metal flows into the connection area.

[0056] (6) Flowing water cooling: Observe the filling of molten metal through the casting riser. After the riser is filled with molten metal, fill the water cooling tank with water to cool the steel claws.

[0057] (7) Repair treatment: After the self-propagating casting is completed, the mold is removed, the gate and riser metal are cut off, and the metal overflowing around the mold is cleaned.

[0058] Example 2

[0059] This embodiment provides a method for vertically connecting an anode steel claw and an anode aluminum guide rod of an electrolytic cell, including the following steps (eg Figure 1 ):

[0060] (1) Steel claw casting and welding: Use the lost foam casting method to cast the Q235 anode steel claw beam and steel claw foot, and weld the steel claw to the beam.

[0061] (2) Surface treatment of the steel claw boss: A T-shaped protrusion with a height of 150 mm and a length of 200 mm is welded on the surface of the steel claw boss, and the surface of the steel claw boss is roughened by sandblasting (such as Figure 5 ).

[0062] (3) Docking and positioning of self-propagating casting parts: Degrease and descaling the connecting end of the aluminum guide rod, place the steel claw in a water-free water cooling tank, with the water level 12 cm below the upper plane of the steel claw beam. Hoist the guide rod and align it with the connecting end of the steel claw boss, with a distance of 35 cm between the two welding end faces.

[0063] (4) Preparation for self-propagating melting and casting: Place the self-propagating melting and casting mold around the connection between the aluminum guide rod and the steel claw boss, and ensure that the gate mold and the riser mold are placed in alignment. Use refractory clay to fix the mold and fill the gap between the molds. Open a hole at the bottom of the self-propagating melting and casting crucible and cover it with a 12mm diameter and 3mm thick pure aluminum sheet. Prepare the self-propagating melting and casting raw material powder, which can be: 23% iron oxide, 6% copper oxide, 1.5% manganese oxide, 9% tin dioxide, 11% calcium sulfate, 6% magnesium sulfate, 5% barium sulfate, the minimum mass percentage of the above materials is not less than 50%, 4% calcium fluoride, 0.25% lanthanide oxide, 4% silicon powder, 24% 300 mesh aluminum powder, and the rest is 100 mesh aluminum powder. Mix them evenly and place them in the self-propagating melting and casting crucible. Preheat the self-propagating melting and casting mold and the steel claw boss.

[0064] (5) Self-propagating casting: After the steel claw boss is preheated to 700°C, a self-propagating casting crucible is placed, the self-propagating casting powder is ignited, a self-propagating reaction occurs, and the molten metal flows into the connection area.

[0065] (6) Flowing water cooling: Observe the filling of molten metal through the casting riser. After the riser is filled with molten metal, fill the water cooling tank with water to cool the steel claws.

[0066] (7) Repair treatment: After the self-propagating casting is completed, the mold is removed, the gate and riser metal are cut off, and the metal overflowing around the mold is cleaned.

[0067] Example 3

[0068] A method for vertically connecting an anode steel claw and an anode aluminum guide rod of an electrolytic cell, comprising the following steps (eg Figure 1 ):

[0069] (1) Steel claw casting and welding: Use the sand casting method to cast the Q235 anode steel claw beam and steel claw foot, and weld the steel claw to the beam.

[0070] (2) Surface treatment of the steel claw boss: Drill three holes with a depth of 50 mm and a diameter of 20 mm on the surface of the steel claw boss, and use a grinding wheel to roughen the surface of the steel claw boss (such as Figure 6 ).

[0071] (3) Docking and positioning of self-propagating casting parts: Degrease and descaling the connecting end of the aluminum guide rod, place the steel claw in a water-free water cooling tank, with the water level 12 cm below the upper plane of the steel claw beam. Hoist the guide rod and align it with the connecting end of the steel claw boss, with a distance of 35 cm between the two welding end faces.

[0072] (4) Preparation for self-propagating melting and casting: Place the self-propagating melting and casting mold around the connection between the aluminum guide rod and the steel claw boss, and ensure that the gate mold and the riser mold are placed in alignment. Use refractory clay to fix the mold and fill the gap between the molds. Open a hole at the bottom of the self-propagating melting and casting crucible and cover it with a pure aluminum sheet with a diameter of less than 15 mm and a thickness of less than 5 mm. Prepare the self-propagating melting and casting raw material powder, which can be: 21% iron oxide, 6% copper oxide, 1% manganese oxide, 9% tin dioxide, 9% calcium sulfate, 4% magnesium sulfate, 3.5% barium sulfate, 2.5% calcium fluoride, 0.2% lanthanide oxide, 4% silicon powder, 24% 300 mesh aluminum powder, and the rest is 100 mesh aluminum powder. Mix them evenly and place them in the self-propagating melting and casting crucible. Preheat the self-propagating melting and casting mold and the steel claw boss.

[0073] (5) Self-propagating casting: After the steel claw boss is preheated to 750°C, a self-propagating casting crucible is placed, the self-propagating casting powder is ignited, a self-propagating reaction occurs, and the molten metal flows into the connection area.

[0074] (6) Flowing water cooling: Observe the filling of molten metal through the casting riser. After the riser is filled with molten metal, fill the water cooling tank with water to cool the steel claws.

[0075] (7) Repair treatment: After the self-propagating casting is completed, the mold is removed, the gate and riser metal are cut off, and the metal overflowing around the mold is cleaned.

[0076] Comparative Example

[0077] This comparative example provides a method of using traditional aluminum-steel explosion blocks to transitionally weld steel claws and aluminum guide rods:

[0078] The first step is to process the welding grooves around the aluminum guide rod and the anode steel claws to be welded, and clean and grind the processed surface and the surface to be welded.

[0079] The second step is to lay the aluminum guide rod and the anode steel claw horizontally, place the aluminum-steel explosion block between the two, clean the end faces of the aluminum guide rod, the anode steel claw and the aluminum-steel explosion block, and use carbon dioxide gas shielded welding to weld the interface between the aluminum-steel explosion block and the steel claw, that is, steel-steel welding.

[0080] The third step is to use carbon dioxide gas shielded welding to weld the interface between the aluminum-steel explosion block and the aluminum guide rod, that is, aluminum-aluminum welding.

[0081] Application performance testing

[0082] The performance of the anode conductive parts of the electrolytic aluminum process prepared in Examples 1-3 and the comparative example was tested. In Example 1, a total of 4 sets of connectors were made, all of which were tried out in the second phase plant of a Ningxia aluminum industry group, and the use effect was good; Examples 2 and 3 each made 1 set of connectors, and the relevant tests were carried out in the laboratory. The test results of the hanging slot pressure drop are shown in Table 2 below.

[0083] Table 2

[0084] Example 1 Example 2 Example 3 Comparative Example Hanging slot voltage drop / mV 40.28 50 48 58.22

[0085] As can be seen from the above table,

[0086] In the comparative example, the traditional method uses an aluminum-steel explosion block to connect the aluminum guide rod and the anode steel claw. The final product has three interfaces, namely the aluminum-steel interface of the aluminum-steel explosion block, the steel-steel welding interface and the aluminum-aluminum welding interface. Affected by multiple interfaces, the voltage drop is relatively high, reaching 58.22mV.

[0087] In the embodiment 1-3, the connecting piece formed by the method of vertically connecting the anode steel claw and the anode aluminum guide rod of the electrolytic cell provided by the present invention has a significantly lower average pressure drop than the traditional explosive block connection method, which can reduce energy consumption in electrolytic aluminum production, and the minimum hanging tank pressure drop is only 40.28mV. At the same time, the connection method also has the advantages of simple process and low production cost, and is easy to promote and apply.

[0088] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for vertically connecting an anode steel claw and an anode aluminum guide rod of an electrolytic cell, characterized in that: The following steps are involved: S1. Roughening the surface of the steel claw boss of the anode steel claw, and then placing the anode steel claw vertically; S2, pre-treating the connecting end of the aluminum guide rod, and vertically hanging the aluminum guide rod above the steel claw boss, so that a welding gap is left between the connecting end and the steel claw boss; S3, surrounding the casting mold around the connection end, the welding gap and the outer side of the steel claw boss, fixing the casting mold and filling the connection gap, placing self-propagating casting powder, and preheating the casting mold and the steel claw boss; the casting mold includes: a gate mold, a riser mold, a front plugging mold and a rear plugging mold; a self-propagating crucible is placed in the gate mold, and the self-propagating casting powder is contained in the self-propagating crucible; S4, when the steel claw boss is preheated to 650-800°C, the self-propagating casting powder in the casting mold is ignited to allow the molten metal to flow into and fill the welding gap; The components of the self-propagating melting casting powder are calculated by mass fraction: 20% to 23% iron oxide, 4% to 6% copper oxide, 1% to 1.5% manganese oxide, 8% to 9% tin dioxide, 9% to 11% calcium sulfate, 4% to 6% magnesium sulfate, 3% to 5% barium sulfate, and the total mass fraction of the foregoing components is not less than 50%; and 2.5% to 4% calcium fluoride, 0.2% to 0.25% lanthanide oxide, 4% silicon powder, 22% to 24% 300 mesh aluminum powder, and the rest is 100 mesh aluminum powder; S5. Use water cooling to directly cool the steel claws and indirectly cool the connection parts. The maximum water filling height is located 10~15cm below the upper plane of the steel claw beam; then remove the mold and perform shaping on the connection parts to complete the vertical connection of the anode steel claws and the anodized aluminum guide rods.

2. The method according to claim 1, characterized in that In step S1, a protrusion and / or a recessed structure is provided on a side of the steel claw boss facing the connecting end.

3. The method according to claim 1, characterized in that: In step S2, the pretreatment includes degreasing and descaling.

4. The method according to claim 1, characterized in that: In step S2, the height of the welding gap is 30-40 cm.

5. The method according to claim 1, characterized in that In step S3, refractory clay is used to fix each mold, and refractory clay is used to fill the gaps between each mold and the connecting end, each mold and the steel claw boss, and between each mold.

6. An anode conductive component for an electrolytic aluminum process, comprising an anode aluminum guide rod and an anode steel claw, characterized in that: The anode aluminum guide rod and the anode steel claw are connected by the method according to any one of claims 1-5.