A method for preparing protein fibers with controllable surface charge and its application.

By cross-linking with glutaraldehyde-based cross-linking agents and controlling surface charge through acid washing, stable protein fibers were prepared, solving the problems of uncontrollable charge and poor stability in existing technologies. This method enables broad-spectrum removal of pollutants of different properties and reduces costs.

CN116770449BActive Publication Date: 2026-11-17SUN YAT SEN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210243491.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-11
Publication Date
2026-11-17
Estimated Expiration
2042-03-11

AI Technical Summary

Technical Problem

In the preparation process of existing protein fibers, the surface charge is uncontrollable, resulting in limited adsorption effect on pollutants of different properties in the environment, poor stability, high cost of designing and expressing specific proteins, and difficulty in achieving mass production.

Method used

By using water-soluble protein spinning followed by cross-linking with glutaraldehyde-based cross-linking agents to form stable protein fibers, and then adjusting their surface charge through acid washing, negatively or positively charged protein fibers can be prepared.

Benefits of technology

It achieves broad-spectrum removal of positively charged, negatively charged, or neutral pollutants in the environment, improves the water stability and tensile properties of fibers, reduces preparation costs, and simplifies operation steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116770449B_ABST
    Figure CN116770449B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing protein fibers with controllable surface charge and its applications. The invention involves cross-linking existing protein spinning with a glutaraldehyde-based cross-linking agent, transforming the originally water-soluble protein fibers into water-insoluble, stable fibers, thus improving their water stability. Further, acid washing with an acid capable of hydrolyzing amide bonds allows for the control of the surface charge of the protein fibers. The preparation process of the protein fibers described in this invention does not require specific protein design and expression, and has advantages such as simple operation and low cost. By controlling the surface charge of the prepared protein fibers, a broad spectrum of removal of positively charged, negatively charged, or neutral pollutants in the environment can be achieved, showing great application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of protein fiber manufacturing and processing technology. More specifically, it relates to a method for preparing protein fibers with controllable surface charge and its application. Background Technology

[0002] Protein fiber is a category of man-made fibers, referring to fibers made from proteins extracted from natural sources such as milk, soybeans, peanuts, and corn, dissolved in appropriate solvents. As early as 1866, the Englishman E.E. Hughes successfully produced man-made protein fibers by coagulating an acetic acid solution of animal glue in an aqueous solution of nitrates and then spinning it into fibers. In 1935, the Italian Fredi followed suit, using casein to create artificial wool. While the resulting artificial wool was less soft than natural wool, it was less prone to wrinkles, insects, and was easier to preserve. Subsequently, various types of man-made protein fibers continued to develop and gradually achieved industrialized production.

[0003] Currently, the potential negative impacts of microplastics and numerous organic pollutants in global water resources on aquatic ecosystems and human health have attracted widespread attention. How to effectively monitor, analyze, and solve water pollution problems has become a common challenge facing society and the world. With the development of science and technology and people's pursuit of a better life, the application of protein fibers is no longer limited to textiles; the idea of ​​using protein fibers for continuous water purification is gradually becoming a reality. For example, Yuan et al. fused the super uranyl-binding protein gene with the spider protein gene to synthesize a chimeric spider protein-based super uranyl-binding protein fiber. This fiber achieved a breakthrough uranium extraction capacity of 12.33 mg g / kg from seawater. -1 Or it could be a promising adsorbent for uranium extraction from natural seawater (Yuan Y, Yu Q, Wen J, Li C, Guo Z, Wang X, Wang N. Ultrafast and highly selective uranium extraction from seawater by hydrogel-like spidroin-based protein fiber. Angew. Chem. Int. Ed. 2019, 58, 11785.). Peydayesh et al. used amyloid fibrils prepared from β-lactoglobulin, the main component of whey protein, as the basis for preparing aerogels. The resulting amyloid fibril aerogels showed good removal effects on metribuzin, ibuprofen, and bisphenol A (Peydayesh M, Suter M, Bolisettty S, Boulos S, Handschin S, L, Mezzenga R. Amyloid fibrils aerogel for sustainable removal of organic contaminants from water. Adv. Mater. 2020, 1907932. This indicates that the field of environmental water pollution control using protein fibers as adsorbents is emerging.

[0004] Traditional protein fiber preparation methods typically only consider fiber formation and post-formation stability. Protein fibers prepared using existing proteins can only adsorb certain environmental pollutants and exhibit poor stability. For example, β-lactoglobulin, which carries a negative charge in neutral aqueous solutions, only exhibits adsorption capacity for positively charged or near-neutral pollutants when spun into β-lactoglobulin fibers; it cannot remove negatively charged pollutants. Other studies are exploring novel specific proteins to adsorb specific targets in the environment, but the design and expression of specific proteins are expensive, purification steps are time-consuming and laborious, and mass production is difficult. Therefore, from both a manufacturing cost and practical environmental perspective, providing protein fibers with controllable surface charge is crucial for achieving broad-spectrum removal of pollutants with diverse properties from the environment. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to overcome the defects and deficiencies of the existing technologies and to provide a method for preparing protein fibers with controllable surface charge and its application.

[0006] The first objective of this invention is to provide a method for preparing protein fibers with controllable surface charge.

[0007] A second objective of this invention is to provide a protein fiber with controllable surface charge.

[0008] A third objective of this invention is to provide the application of the protein fiber in water pollution control.

[0009] The above-mentioned objective of this invention is achieved through the following technical solution:

[0010] The present invention comprises the following steps:

[0011] S1. Prepare spinning solution using water-soluble protein;

[0012] S2. Spinning; The spinning solution from step S1 is squeezed from the spinneret into the coagulation bath to obtain wet protein fibers; collected and dried to obtain dry protein fibers.

[0013] S3. Crosslinking protein fibers; The dried protein fibers obtained in step S2 are subjected to a crosslinking reaction with a glutaraldehyde-based crosslinking agent. After the reaction is complete, excess crosslinking agent is washed off, and the fibers are dried to obtain negatively charged protein fibers.

[0014] S4. Acid washing; The negatively charged protein fibers obtained in step S3 are placed in an acid solution, shaken, washed, and dried to obtain positively charged protein fibers.

[0015] Specifically, the protein mentioned in step S1 is bovine serum albumin (BSA).

[0016] Specifically, in step S1, a spinning solution is prepared by dissolving the protein in a Tris buffer solution with a concentration of 10-30 mM and a pH of 8-9; the concentration of the protein in the spinning solution is 100-500 mg / mL.

[0017] Preferably, the concentration of protein in the spinning solution is 240–350 mg / mL, as shown in Example 8.

[0018] Specifically, the coagulation bath in step S2 is ethanol, methanol, or acetone.

[0019] Specifically, in step S2, spinning is performed using an injection pump with a spinneret flow rate of 4–20 μL / min.

[0020] Preferably, the spinneret flow rate is 6–12 μL / min, as shown in Example 8.

[0021] Specifically, the drying process described in step S2 is room temperature vacuum drying.

[0022] Specifically, the glutaraldehyde-based crosslinking agent mentioned in step S3 is genipin (GP). Genipin contains a glutaraldehyde structure within its molecule, which can spontaneously react with amino groups, and its toxicity is much lower than that of glutaraldehyde. When preparing the crosslinking agent solution, its amount is calculated based on the amount of amino groups contained in the dried protein fibers obtained in step S2. Specifically, if the amount of amino groups contained in the protein fibers is n, then the amount of crosslinking agent required should be greater than 1n.

[0023] Preferably, the amount of the crosslinking agent is 1.5 to 3n, as shown in Example 8.

[0024] Taking the cross-linking reaction using genipin solution as an example; specifically, genipin is dissolved in an appropriate amount of ethanol to obtain a genipin solution, and then the dry protein fiber obtained in step S2 is completely immersed in the prepared genipin solution to allow the cross-linking reaction to occur. After the reaction is completed, excess cross-linking agent is washed away with ethanol, and the washed fiber is dried to obtain a water-stable protein fiber with a negatively charged surface.

[0025] Specifically, the cross-linking reaction was carried out at a temperature of 37°C for 12 hours.

[0026] Specifically, the concentration of the crosslinking agent genipin solution is 0.01–0.05 g / mL.

[0027] Specifically, the acid solution in step S4 is an acid that can hydrolyze amide bonds, and its concentration is 0.1 to 6 mol / L.

[0028] Specifically, the acid solution is hydrochloric acid.

[0029] Preferably, the concentration of the hydrochloric acid is 1-6 mol / L, as shown in Example 8.

[0030] Preferably, the pickling and oscillation time in step S4 is 2 to 12 hours, as shown in Example 8.

[0031] The present invention also seeks to protect the protein fibers prepared by the above method, including the negatively charged protein fibers prepared in step S3 and the positively charged protein fibers prepared in step S4.

[0032] This invention uses bovine serum albumin (BSA) as an example to prepare protein fibers (BSA fiber), which are water-soluble, meaning they are unstable in water. To improve the water stability of BSA fiber, this invention utilizes glutaraldehyde-based crosslinking agents, such as genipin, to crosslink the amine groups on the BSA fiber with the aldehyde groups on the crosslinking agent, resulting in an aldehyde-amine condensation reaction. This crosslinks the water-soluble BSA fiber into a stable fiber that is insoluble in water, thus improving its water stability and tensile properties. Furthermore, after crosslinking with genipin, some hydroxyl groups inherent in genipin itself further enhance the overall hydrophilicity of the fiber. Since the protein obtained after genipin crosslinking is generally dark green, the color can be used as a preliminary indication of successful crosslinking, facilitating observation.

[0033] Because BSA fiber itself contains many amide bonds, the cross-linked CBSA fiber(-) also generates some new amide bonds. This invention utilizes acid washing with hydrolyzable amide bonds to hydrolyze these bonds into carboxyl groups and positively charged ammonium salts, thus controlling the charge of the CBSA fiber(-) and obtaining positively charged CBSA fiber(+). Furthermore, the acid-washed CBSA fiber(+) still exhibits good water stability. Both the negatively charged and positively charged protein fibers prepared by this invention possess excellent adsorption properties and can broadly remove positively charged, negatively charged, or neutral pollutants from the environment. Therefore, this invention also seeks protection for the application of the aforementioned protein fibers in water pollution control.

[0034] The present invention has the following beneficial effects:

[0035] This invention transforms existing water-soluble protein fibers into stable, water-insoluble fibers by cross-linking them with a glutaraldehyde-based cross-linking agent, thereby improving their water stability. Further, acid washing with an acid capable of hydrolyzing amide bonds allows for the control of the surface charge of the protein fibers. The preparation process of the surface-charge-controllable protein fibers described in this invention does not require specific protein design and expression. The surface charge of the protein fibers can be controlled through a simple acid washing step after cross-linking, offering advantages such as ease of operation and low cost. Furthermore, by controlling the surface charge of the prepared protein fibers, a broad spectrum of removal of positively, negatively, or neutral pollutants in the environment can be achieved, demonstrating promising application prospects. Attached Figure Description

[0036] Figure 1 The diagram shows the fabrication process of CBSA fiber, along with scanning electron microscope images and water stability test results of the corresponding fibers.

[0037] Figure 2 Stress curves for CBSA fiber(-) and CBSA fiber(+).

[0038] Figure 3 Thermogravimetric analysis diagrams of BSA, BSA fiber, CBSA fiber(-), and CBSA fiber(+).

[0039] Figure 4 The zeta potential diagrams are for BSA fiber, CBSA fiber(-), and CBSA fiber(+).

[0040] Figure 5 The surface potential distribution diagrams are shown for BSA fiber, CBSA fiber(-), and CBSA fiber(+).

[0041] Figure 6 The images show the circular dichroism chromatograms of BSA and BSA fiber, and the secondary structures obtained by fitting the data according to Young's equation.

[0042] Figure 7 This represents the water contact angle between BSA and BSA fiber.

[0043] Figure 8 The results are based on molecular dynamics calculations of BSA in aqueous and ethanol solutions.

[0044] Figure 9 The diagram shows the reaction process of CBSA fiber(-) and CBSA fiber(+).

[0045] Figure 10Infrared spectra of BSA, BSA fiber, CBSA fiber(-), and CBSA fiber(+).

[0046] Figure 11 XPS spectra of O1s and N1s for BSA fiber, CBSA fiber(-), and CBSA fiber(+).

[0047] Figure 12 Comparison of CBSA fiber(-) and CBSA fiber(+) before and after removal of dyes with different charges.

[0048] Figure 13 Figure 1 shows the removal efficiency of CBSA fiber(-) and CBSA fiber(+) for dyes with different charges. Figure 2 shows the removal efficiency of CBSA fiber(-) for methylene blue, rhodamine 6G and methyl green. Figure 3 shows the removal time of CBSA fiber(-) for methylene blue, rhodamine 6G and methyl green. Figure 4 shows the removal efficiency of CBSA fiber(+) for erythrosine B, mordant blue 29 and methylene blue. Figure 5 shows the removal time of CBSA fiber(+) for erythrosine B, mordant blue 29 and methylene blue.

[0049] Figure 14 The structure and charge of the emerging organic pollutants being tested.

[0050] Figure 15 The figures show the removal efficiency of CBSA fiber(-) and CBSA fiber(+) for different types of organic pollutants. Figure a shows the removal efficiency of CBSA fiber(-) for 1-NO, 1-NA, OPD, BPA, BPS, and PH; Figure b shows the removal time of CBSA fiber(-) for 1-NO, 1-NA, OPD, BPA, BPS, and PH; Figure c shows the removal efficiency of CBSA fiber(+) for PFOA and PFOS; and Figure d shows the removal time of CBSA fiber(+) for PFOA and PFOS.

[0051] Figure 16 The Langmuir adsorption isotherms of CBSA fiber(-) and CBSA fiber(+) for different types of organic pollutants are shown in Figures a to f. The Langmuir adsorption isotherms of CBSA fiber(-) for 1-NO, 1-NA, OPD, BPA, BPS and PH are shown in Figures g to h.

[0052] Figure 17 The results of 4 cycles of methylene blue removal by CBSA fiber(-) and CBSA fiber(+) are shown. Detailed Implementation

[0053] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.

[0054] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.

[0055] The ethanol (EtOH) used in this invention was supplied by Maclean Biotech Co., Ltd. (Guangdong, China); the hydrochloric acid used was purchased from Guangzhou Chemical Reagent Co., Ltd. (Guangdong, China); the 1-naphthol (1-NO), 1-naphthylamine (1-NA), bisphenol A (BPA), bisphenol S (BPS), 1,2-phenylenediamine (OPD), methylene blue, rhodamine 6G, methyl green, erythrosine B, mordant blue 29, and methylene blue used were purchased from Aladdin Chemical Co., Ltd. (Shanghai, China); the bovine serum albumin (BSA) used was purchased from Beijing Bailingwei Technology Co., Ltd. (Beijing, China); the genipin (GP) used was purchased from Beijing Anaiji Energy Engineering Technology Co., Ltd. (Beijing, China); the DL-propranolol hydrochloride (PH) used was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd. (Shanghai, China); and the perfluorooctanoic acid (PFOA) and perfluorooctyl sulfonic acid (PFOS) used were purchased from AccuStandard (USA).

[0056] Example 1: Preparation of protein fibers with controllable surface charge

[0057] 1.50 g of bovine serum albumin (BSA) was dissolved in 5 mL of Tris buffer (pH = 8.8, 20 mM) to obtain a bovine serum albumin solution with a concentration of 300 mg / mL (spinning solution). Under the action of a syringe pump, the 300 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 8 μL / min to obtain wet bovine serum albumin fibers (BSA fiber). The wet BSA fiber was then collected and dried under vacuum at room temperature to obtain dry BSA fiber.

[0058] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:2 (molar amount of amino groups in BSA fiber to molar amount of GP). Based on calculations, 0.67 g of GP powder was weighed and added to 20 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -22.17 mV using a zeta potential meter.

[0059] The CBSA fiber(-) was placed in a 1 mol / L hydrochloric acid solution and shaken for 12 h, then washed with ultrapure water to remove the hydrochloric acid. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be 23.32 mV using a zeta potential meter.

[0060] Example 2: Preparation of protein fibers with controllable surface charge

[0061] 1.25 g of bovine serum albumin was dissolved in 5 mL of Tris buffer (pH = 8, 30 mM) to obtain a bovine serum albumin solution with a concentration of 240 mg / mL (spinning solution); under the action of a syringe pump, the 240 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 12 μL / min to obtain wet bovine serum albumin fibers (BSA fiber); then, the wet BSA fiber was collected and dried under vacuum at room temperature to obtain dry BSA fiber.

[0062] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:2 (molar amount of amino groups in the BSA fiber to molar amount of GP). Based on calculations, 0.67 g of GP powder was weighed and added to 20 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -26.86 mV using a zeta potential meter.

[0063] The CBSA fiber(-) was placed in a 1 mol / L hydrochloric acid solution and shaken for 12 h, then washed with ultrapure water to remove the hydrochloric acid. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be 24.63 mV using a zeta potential meter.

[0064] Example 3: Preparation of protein fibers with controllable surface charge

[0065] 1.75 g of bovine serum albumin was dissolved in 5 mL of Tris buffer (pH = 9, 30 mM) to obtain a bovine serum albumin solution with a concentration of 350 mg / mL (spinning solution); under the action of a syringe pump, the 350 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 6 μL / min to obtain wet bovine serum albumin fibers (BSA fiber); then, the wet BSA fiber was collected and dried under vacuum at room temperature to obtain dry BSA fiber.

[0066] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:2 (molar amount of amino groups in BSA fiber to molar amount of GP). Based on calculations, 0.67 g of GP powder was weighed and added to 20 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -25.18 mV using a zeta potential meter.

[0067] The CBSA fiber(-) was placed in a 1 mol / L hydrochloric acid solution and shaken for 12 h, then washed with ultrapure water to remove the hydrochloric acid. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be 27.46 mV using a zeta potential meter.

[0068] Example 4: Preparation of protein fibers with controllable surface charge

[0069] 1.50 g of bovine serum albumin was dissolved in 5 mL of Tris buffer (pH = 8, 20 mM) to obtain a bovine serum albumin solution with a concentration of 300 mg / mL (spinning solution); under the action of a syringe pump, the 300 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 8 μL / min to obtain wet bovine serum albumin fibers (BSA fiber); then, the wet BSA fiber was collected and dried under vacuum at room temperature to obtain dry BSA fiber.

[0070] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:1.5 (molar amount of amino groups in BSA fiber to molar amount of GP). Based on calculations, 0.50 g of GP powder was weighed and added to 15 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -20.15 mV using a zeta potential meter.

[0071] The CBSA fiber(-) was placed in a 1 mol / L hydrochloric acid solution and shaken for 12 h, then washed with ultrapure water to remove the hydrochloric acid. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be 25.66 mV using a zeta potential meter.

[0072] Example 5: Preparation of protein fibers with controllable surface charge

[0073] 1.50 g of bovine serum albumin was dissolved in 5 mL of Tris buffer (pH = 8.8, 20 mM) to obtain a bovine serum albumin solution with a concentration of 300 mg / mL (spinning solution); under the action of a syringe pump, the 300 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 8 μL / min to obtain wet bovine serum albumin fibers (BSA fiber); then, the wet BSA fiber was collected and dried under vacuum at room temperature to obtain dry BSA fiber.

[0074] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:3 (molar amount of amino groups in BSA fiber to molar amount of GP). Based on calculations, 1.01 g of GP powder was weighed and added to 30 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -25.23 mV using a zeta potential meter.

[0075] The CBSA fiber(-) was placed in a 1 mol / L hydrochloric acid solution and shaken for 12 h, then washed with ultrapure water to remove the hydrochloric acid. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be -24.88 mV using a zeta potential meter.

[0076] Example 6: Preparation of protein fibers with controllable surface charge

[0077] 0.5 g of bovine serum albumin was dissolved in 5 mL of Tris buffer (pH = 8, 10 mM) to obtain a bovine serum albumin solution with a concentration of 100 mg / mL (spinning solution); under the action of a syringe pump, the 100 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 8 μL / min to obtain wet bovine serum albumin fibers (BSA fibers); then, the wet BSA fibers were collected and dried under vacuum at room temperature to obtain dry BSA fibers.

[0078] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:2 (molar amount of amino groups in the BSA fiber to molar amount of GP). Based on calculations, 0.67 g of GP powder was weighed and added to 20 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -26.92 mV using a zeta potential meter.

[0079] The CBSA fiber(-) was placed in a 1 mol / L hydrochloric acid solution and shaken for 2 hours. The hydrochloric acid was then washed away with ultrapure water. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be 16.12 mV using a zeta potential meter.

[0080] Example 7: Preparation of protein fibers with controllable surface charge

[0081] 1.50 g of bovine serum albumin was dissolved in 5 mL of Tris buffer (pH = 8.8, 20 mM) to obtain a bovine serum albumin solution with a concentration of 300 mg / mL (spinning solution); under the action of a syringe pump, the 300 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 8 μL / min to obtain wet bovine serum albumin fibers (BSA fiber); then, the wet BSA fiber was collected and dried under vacuum at room temperature to obtain dry BSA fiber.

[0082] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:2 (molar amount of amino groups in BSA fiber to molar amount of GP). Based on calculations, 0.67 g of GP powder was weighed and added to 20 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -22.17 mV using a zeta potential meter.

[0083] The CBSA fiber(-) was placed in a 6 mol / L hydrochloric acid solution and shaken for 12 h, then washed with ultrapure water to remove the hydrochloric acid. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be 30.01 mV using a zeta potential meter.

[0084] Example 8: Preparation of protein fibers with controllable surface charge

[0085] 2.50 g of bovine serum albumin was dissolved in 5 mL of Tris buffer (pH = 8.8, 20 mM) to obtain a bovine serum albumin solution with a concentration of 500 mg / mL (spinning solution); under the action of a syringe pump, the 500 mg / mL bovine serum albumin solution was extruded from a 0.25 mm spinneret into anhydrous ethanol solution at a flow rate of 8 μL / min to obtain wet bovine serum albumin fibers (BSA fiber); then, the wet BSA fiber was collected and dried under vacuum at room temperature to obtain dry BSA fiber.

[0086] 120 mg of dried BSA fiber was taken, and a cross-linking agent was added at a ratio of 1:2 (molar amount of amino groups in BSA fiber to molar amount of GP). Based on calculations, 0.67 g of GP powder was weighed and added to 20 mL of anhydrous ethanol. After ultrasonic dissolution, the GP solution was added to 120 mg of dried BSA fiber, and the reaction was carried out at 37 °C for 12 h. After the reaction, excess cross-linking agent was washed away with ethanol. The washed fiber was dried to obtain water-stable bovine serum albumin fiber (CBSAfiber(-)) with a negatively charged surface. The potential of CBSA fiber(-) was measured to be -22.17 mV using a zeta potential meter.

[0087] The CBSA fiber(-) was immersed in a 0.5 mol / L hydrochloric acid solution and shaken for 12 h, then washed with ultrapure water to remove the hydrochloric acid. Finally, it was vacuum dried to obtain water-stable bovine serum albumin fiber (CBSA fiber(+)) with a positively charged surface. The potential of the CBSA fiber(+) was measured to be 14.66 mV using a zeta potential meter.

[0088] Test Example 1

[0089] To further demonstrate and apply the surface charge controllable protein fibers prepared according to the present invention, the preparation parameters of the above-mentioned surface charge controllable protein fibers are summarized as shown in Table 1:

[0090] Table 1. Specific implementation parameters of a protein fiber with controllable surface charge.

[0091]

[0092] As shown in Table 1, after acid washing, the surface charge of the protein fibers in all embodiments of the present invention can be modulated from negative to positive. The following section details the specific characterization and application of the protein fibers prepared in Example 1.

[0093] This invention utilizes a SU8010 field emission scanning electron microscope (Hitachi, Japan) to obtain scanning electron microscope images; a DSA100 droplet shape analyzer (Kruss, Germany) to obtain water contact angle images; a TG 209F3 Tarsus thermogravimetric analyzer (Netzsch, Germany) to perform thermogravimetric analysis; a Thermo-VG Scientific spectrometer (ESCALAB 250, USA) to obtain X-ray photoelectron spectroscopy (XPS) spectra; a Dimension Fastscan scanning probe microscope (Bruker, Germany) to determine surface potential; a LIFM-nanoparticle size zeta potential and molecular weight analyzer (Brookhaven, USA) to obtain zeta potential; a PerkinElmer Frontier thermogravimetric spectrometer (PerkinElmer, USA) to obtain infrared spectra; a UV2800S UV-Vis spectrophotometer (Sunny Optical, China) to obtain ultraviolet spectra; and an F97... Fluorescence spectra were obtained using a Pro fluorescence spectrophotometer (LengGuang, China); circular dichroism spectra were obtained using a J1700 circular dichroism spectrometer (Jasco, Japan); stress-strain curves were obtained using a ZWICK Z250 electronic universal testing machine (ZWICK, Germany); the concentrations of target organic compounds (1-NO, 1-NA, BPA, BPS, and OPD) were analyzed using HPLC (Shimadzu LC20AD) and a diode array detector (PDA); the concentrations of target organic compounds (PFOA and PFOS) were analyzed using HPLC (Shimadzu LC20AD) and mass spectrometry (ESI source); and a Poroshell 120EC-C18 column (4.6 x 100 mm, 2.7 μm, Agilent Technology, USA) was used.

[0094] 1. Preparation process and basic characterization

[0095] The flowchart of the preparation of the surface charge controllable protein fiber in Example 1 of this invention is as follows: Figure 1 As shown, it also includes scanning electron microscope images of the corresponding fibers and water stability test results. From Figure 1 Scanning electron microscopy (SEM) results showed that the diameter of the dried BSA fiber obtained by room-temperature vacuum drying was approximately 30 μm. Water stability tests indicated that the BSA fiber at this stage was water-soluble, meaning it was unstable in water. However, the CBSA fiber(-) obtained after GP crosslinking exhibited good water stability. Furthermore, the CBSA fiber(+) obtained after acid washing also showed good water stability.

[0096] The stress-strain curves of CBSA fiber(-) and CBSA fiber(+) are as follows: Figure 2As shown, the thermogravimetric analysis results of BSA, BSA fiber, CBSA fiber(-), and CBSA fiber(+) are as follows: Figure 3 As shown. By Figure 2 The stress-strain curves shown are Figure 3 The thermogravimetric analysis results show that the CBSA fiber(-) and CBSA fiber(+) prepared in this invention have excellent thermal stability and tensile properties, and are suitable for the purification of pollutants in water.

[0097] 2. Electrical testing

[0098] The zeta potential diagrams for BSA fiber, CBSA fiber(-), and CBSA fiber(+) are shown below. Figure 4 As shown. By Figure 4 It can be seen that the zeta potentials of BSA fiber and CBSA fiber(-) are -20.45mV and -22.17mV, respectively. Notably, after acid washing with 1mol / L hydrochloric acid solution, the potential of the resulting CBSA fiber(+) changed significantly from -22.17mV to -23.32mV, preliminarily indicating that the acid washing process significantly altered the overall electrical properties of the fiber.

[0099] To provide a microscopic perspective, this invention also included surface potential measurements using atomic force microscopy. In physics, the potential at infinity is defined as zero. The electric field lines around a positive charge are all upstream of infinity, resulting in a positive potential; conversely, the potential around a negative charge is negative. The magnitude of the potential is relative. First, considering the definition of electric field lines, the direction of the electric field lines for a positive charge points from the point of charge towards infinity, while the opposite is true for a negative point charge. Furthermore, the potential gradually decreases along the direction of the electric field lines. Since the potential at infinity is defined as zero, the electric field lines around a positive charge are all upstream of infinity, resulting in a positive potential, and vice versa for a negative charge. The surface potential distribution diagrams for BSA fiber, CBSA fiber(-), and CBSA fiber(+) are shown below. Figure 5 As shown, by Figure 5 It can be seen that the surface potentials of BSA fiber and CBSA fiber(-) are -500mV and -310mV, respectively; while after acid washing, the surface potential of CBSA fiber(+) is 50mV, an increase of 360mV. It is worth noting that the change in surface potential is uniform, and these results further demonstrate that the charge on the surface of the protein fiber has been successfully regulated.

[0100] 3. Mechanism Research

[0101] The protein used in this invention to prepare protein fibers with controllable surface charge is bovine serum albumin (BSA). BSA has a spherical three-dimensional structure composed of three structurally similar domains. Two subdomains within each domain form a cylindrical structure with opposing slots, and almost all hydrophobic amino acids are embedded within the cylinder, forming a hydrophobic cavity. The hydrophilic side chains are exposed, resulting in excellent solubility in water. Furthermore, BSA has an isoelectric point of 4.7, making it negatively charged in neutral aqueous solutions. After spinning in an ethanol solution, the secondary structure obtained from the circular dichroism chromatogram and Young's calculations is as follows... Figure 6 As shown, Figure 6 The results showed that the α-helix and β-turn angles of the BSA fiber changed. The water contact angle test results for BSA and BSA fiber are as follows: Figure 7 As shown, by Figure 7 It can be seen that the water contact angles of BSA and BSA fiber are 20.2° and 80.88°, respectively, indicating that the hydrophilicity of BSA fiber decreases after spinning in ethanol. This invention also performed molecular dynamics simulations of BSA in aqueous and ethanol solutions, respectively, with results as follows... Figure 8 As shown, by Figure 8 The results show that the secondary structure of BSA changes in ethanol solution, the molecular structure becomes looser, the hydrophobic groups that were originally inside are exposed to the molecular surface, while the distribution of hydrophilic groups on the surface is relatively reduced, and the hydrophilicity decreases. This is consistent with the results of water contact angle and circular dichroism fitting.

[0102] The reaction process of obtaining CBSA fiber(-) by crosslinking BSA fiber with GP and obtaining CBSA fiber(+) by acid washing is as follows: Figure 9 As shown. GP is similar to glutaraldehyde, possessing two aldehyde groups, and the crosslinking process of GP is similar to the aldehyde-amine condensation of glutaraldehyde. This invention utilizes GP to crosslink the amine groups on BSA fiber with the aldehyde groups on GP, ​​resulting in an aldehyde-amine condensation reaction. This crosslinks the water-soluble BSA fiber into a stable fiber that is insoluble in water, improving its water stability. Generally, the protein obtained after GP crosslinking is dark green, so the color can be used as a preliminary indication of successful crosslinking. To further verify this, the infrared spectra of BSA, BSA fiber, CBSA fiber(-), and CBSA fiber(+) were detected, and the results are shown below. Figure 10 As shown, the peak changes of the second-generation amide groups in the infrared spectrum prove that the amide groups have been successfully crosslinked. Furthermore, the XPS spectra of O1s and N1s of BSA fiber, CBSA fiber(-), and CBSA fiber(+) are shown below. Figure 11As shown in the figure. XPS O1s peak analysis results indicate that the -OH groups in the crosslinked CBSAfiber(-) are significantly increased, further proving the successful crosslinking. Figure 11 a). Because the cross-linked amine groups are all positively charged or neutral amino acids, the cross-linked CBSA fiber (-) is still negatively charged.

[0103] The reaction process for obtaining CBSA fiber(+) by acid washing is as follows: Figure 9 As shown. BSA fiber itself contains many amide bonds, and the cross-linked CBSA fiber(-) also generates some new amide bonds. This invention uses acid washing with hydrochloric acid (an acid that can hydrolyze amide bonds) to hydrolyze the amide bonds into carboxyl groups and positively charged ammonium salts, thereby controlling the charge of CBSA fiber(-) and obtaining positively charged CBSA fiber(+). This is confirmed by the XPS spectra of BSA fiber, CBSA fiber(-), and CBSA fiber(+) at O1s and N1s. The XPS O1s peak results show that the number of carboxyl groups in the acid-washed CBSA fiber(+) is significantly increased. Figure 11 a). The N1s peak separation results of XPS show that CBSA fiber(+) exhibits a significant -NH4+ peak. + peak ( Figure 11 b). The above results indicate that after acid hydrolysis, the amide bonds of CBSA fiber(-) are hydrolyzed into carboxyl groups and positively charged ammonium salts, thus yielding positively charged CBSA fiber(+). Furthermore, during the acid washing process, the tryptophan is destroyed, generating humic substances, which further deepens the color of the product.

[0104] 4. Practical Application

[0105] Based on the properties of the CBSA fiber(-) and CBSA fiber(+) prepared according to this invention, this invention selected six dyes with different charges to test the removal performance of CBSA fiber(-) and CBSA fiber(+), and the results are as follows. Figure 12 As shown in the figure. The removal efficiency and removal time of CBSA fiber(-) for methylene blue, rhodamine 6G, and methyl green are shown in the figure. Figure 13 As shown in a and 13b; the removal efficiency and removal time of CBSA fiber(+) for erythrosine B, mordant blue 29, and methylene blue are shown in the figures below. Figure 13 As shown in c and 13d. (By...) Figure 12 , Figure 13The results shown in a and 13b indicate that CBSA fiber(-) exhibits excellent removal capabilities for positively charged methylene blue, rhodamine 6G, and methyl green, with an equilibration time of only 5 minutes. Figure 13 b) The removal effect can also be maintained when the three dyes are mixed together. Figure 12 CBSA fiber(+) exhibits excellent removal capabilities for negatively charged erythrosine B, mordant blue, and methylene blue, with a rapid equilibration time. Figure 12 , Figure 13 (c and 13d). The above results show that the two fibers with different surface charges can achieve rapid removal of organic dyes with different charges in the actual environment.

[0106] In addition to the dyes with different charges mentioned above, this invention also selected eight different types of organic pollutants to evaluate the adsorption performance of CBSA fiber(-) and CBSA fiber(+). The structure and charge of the tested organic pollutants are as follows: Figure 14 As shown in the figure. Among them, 1-NO, 1-NA, OPD, BPA, and BPS are slightly neutral, pH is positively charged, while PFOA and PFOS are negatively charged. The removal effects of CBSA fiber(-) and CBSA fiber(+) on the above different types of organic pollutants are shown in the figure. Figure 15 As shown; where, Figure 15 a is a graph showing the removal efficiency of CBSA fiber(-) for 1-NO, 1-NA, OPD, BPA, BPS, and PH. Figure 15 b is a time-dependent removal plot of 1-NO, 1-NA, OPD, BPA, BPS, and PH by CBSA fiber(-). Figure 15 c is a graph showing the removal efficiency of CBSAfiber(+) for PFOA and PFOS. Figure 15 d is a time-sharing plot of PFOA and PFOS removal by CBSA fiber(+). Figure 15 The removal experiments shown indicate that CBSA fiber(-) has good removal efficiency for neutral 1-NO, 1-NA, OPD, BPA and BPS, as well as positively charged PH.

[0107] It is noteworthy that CBSA fiber(-) exhibits the fastest equilibrium time with positively charged pH, indicating that surface charge is the dominant force. Figure 15 Similarly, CBSA fiber(+) achieved high removal efficiency for negatively charged PFOA and PFOS within 5 minutes, indicating that surface charge plays a decisive role.

[0108] Langmuir adsorption isotherms of CBSA fiber(-) and CBSA fiber(+) for different types of organic pollutants, such as... Figure 16 As shown in the figures; among them, the Langmuir adsorption isotherms of CBSA fiber(-) for 1-NO, 1-NA, OPD, BPA, BPS and PH are shown in Figures a to f in sequence; the Langmuir adsorption isotherms of CBSA fiber(+) for PFOA and PFOS are shown in Figures g to h in sequence. Figure 16 The Langmuir adsorption isotherm fitting results show that the adsorption capacities (Q) of CBSA fiber(-) and CBSA fiber(+) are 108–250 mg / g and 246–258 mg / g, respectively, which are satisfactory. The binding constant (K) values ​​also indicate that both CBSA fiber(-) and CBSA fiber(+) have large binding constants for organic pollutants with opposite charges, further confirming that the main interaction force is the surface charge effect.

[0109] In addition, this invention also tested the recycling of the two fibers. Figure 17 The results of four cycles of methylene blue removal by CBSA fiber(-) and CBSA fiber(+) are presented. For the removal cycle experiment of CBSA fiber(-), methylene blue was used as an example; the adsorbed CBSA fiber(-) was washed with 1 mol / L ammonium acetate methanol solution for 15 minutes, and then rinsed with pure water. Figure 17 As shown in Figure a, the cleaned CBSA fiber(-) maintained a 99% removal efficiency after 4 cycles. For the removal cycle experiment of CBSA fiber(+), methylene blue was used as an example; the adsorbed CBSA fiber(+) was washed with a saturated ammonium chloride methanol solution for 15 minutes, and then rinsed thoroughly with pure water. Figure 17 As shown in b, the cleaned CBSA fiber(+) still maintains a removal efficiency of over 96% after 4 cycles.

[0110] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A method for preparing protein fibers with controllable surface charge, comprising the following steps: S1. Prepare spinning solution using water-soluble protein; S2. Spinning; The spinning solution from step S1 is squeezed from the spinneret into the coagulation bath to obtain wet protein fibers; these fibers are collected and dried to obtain dry protein fibers. S3. Crosslinking protein fibers; The dried protein fibers obtained in step S2 are subjected to a crosslinking reaction with a glutaraldehyde-based crosslinking agent. After the reaction is complete, excess crosslinking agent is washed off, and the fibers are dried to obtain negatively charged protein fibers. S4. Acid washing; The negatively charged protein fibers obtained in step S3 are placed in an acid solution, shaken, washed, and dried to obtain positively charged protein fibers. The water-soluble protein mentioned in step S1 is bovine serum albumin; The glutaraldehyde crosslinking agent mentioned in step S3 is genipin. Its dosage is calculated based on the amount of amino groups contained in the dried protein fiber obtained in step S2. If the amount of amino groups contained in the protein fiber is n, then the amount of crosslinking agent required should be greater than 1n. The acid solution mentioned in step S4 is an acid that can hydrolyze amide bonds, and its concentration is 0.1 to 6 mol / L.

2. The method according to claim 1, characterized in that, In step S1, a spinning solution is prepared by dissolving the protein in a Tris buffer solution with a concentration of 10–30 mM and a pH of 8–9; the concentration of the protein in the spinning solution is 100–500 mg / mL.

3. The method according to claim 1, characterized in that, The coagulation bath in step S2 is ethanol, methanol, or acetone.

4. The method according to claim 1, characterized in that, In step S2, spinning is performed using an injection pump with a spinneret flow rate of 4–20 μL / min.

5. The method according to claim 1, characterized in that, The oscillation time in step S4 is 2 to 12 hours.

6. The protein fibers prepared by any one of claims 1 to 5.

7. The application of the protein fiber according to claim 6 in the prevention and control of organic pollutant water pollution.

Citation Information

Patent Citations

  • Animal blood protein fiber and preparation method thereof

    CN102154731A

  • Fibrous protein adsorption of heavy metals

    US20040124151A1