A lithium iron phosphate positive electrode active material and preparation method thereof, positive electrode sheet and lithium ion battery

By regulating the particle size and sphericity parameters of the lithium iron phosphate material, the mixed cathode active material improves the compaction density and electrochemical performance of the battery, solves the problem of low energy density of the lithium iron phosphate material, and achieves high energy density and Balance of excellent cycle performance.

CN116779777BActive Publication Date: 2024-10-11BYD CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202210228577.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-07
Publication Date
2024-10-11
Estimated Expiration
2042-03-07

AI Technical Summary

Technical Problem

The maximum compacted density of lithium iron phosphate cathode material is small, resulting in a low energy density of the battery, which cannot meet the market demand for high endurance. At the same time, increasing the compacted density will be accompanied by a decrease in electrochemical performance.

Method used

By regulating the particle size and sphericity parameters of the two lithium iron phosphate materials, the mixed cathode active material can achieve high compaction density while maintaining excellent electrochemical performance. Specifically, by limiting the Dmo range and the range of the relevant relationship formula, the mixture is ensured It has high packing density and excellent cycle performance.

Benefits of technology

The compacted density of the positive electrode plate was increased to more than 2.6g/cm3, which improved the energy density of the battery and maintained good cycle performance and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116779777B_ABST
    Figure CN116779777B_ABST
Patent Text Reader

Abstract

The present application provides a lithium iron phosphate positive electrode active material and a preparation method thereof, a positive electrode plate and a lithium ion battery. The positive electrode active material is formed by mixing a first lithium iron phosphate material and a second lithium iron phosphate material, wherein the particle sizes corresponding to the distribution percentages when the volumes of the first and second lithium iron phosphate materials reach the maximum are D 1 mo μm, D 2 mo μm, and 0.3≤D 1 mo ≤3.2, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo The sphericity of the first and second lithium iron phosphate materials are A1 and A2 respectively, and 0.49<0.643D 1 mo +0.439A1<2.3;0.41<1.07D 2 mo +2.44A2‑1.70D 2mo ×A2<1.9. The maximum compaction density of the electrode sheet containing the positive electrode active material can be 2.6g / cm 3 At the same time, the electrochemical performance of the battery is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of lithium-ion batteries, and in particular to a lithium iron phosphate positive electrode active material and a preparation method thereof, a positive electrode sheet and a lithium-ion battery. Background Art

[0002] Lithium iron phosphate materials are widely used due to their advantages such as high safety, low price and environmental friendliness. However, lithium iron phosphate cathode materials have an obvious disadvantage, that is, their maximum compaction density is relatively small (2.1-2.5g / cm 3 ), resulting in low energy density of batteries made from it, which cannot meet the market demand for batteries with long battery life. In order to improve the energy density of batteries, high-density lithium iron phosphate materials are the mainstream development direction in the industry, but while increasing their compaction density, the electrochemical performance of the battery is often reduced. Summary of the invention

[0003] In view of this, the present application provides a lithium iron phosphate positive electrode active material and a preparation method thereof, a positive electrode plate and a lithium ion battery. By regulating the particle size and sphericity parameters of the two lithium iron phosphate materials that constitute it, the compaction density of the positive electrode active material mixed in any proportion can be high, and the electrochemical performance of the battery is relatively good.

[0004] Specifically, in the first aspect, the present application provides a lithium iron phosphate positive electrode active material, which is formed by mixing a first lithium iron phosphate material and a second lithium iron phosphate material, and 0.49<0.643D 1 mo +0.439A1<2.3,0.41<1.07D 2 mo +2.44A2-1.70D 2 mo ×A2<1.9;

[0005] Wherein, the particle size corresponding to the maximum volume distribution percentage of the first lithium iron phosphate material is D 1 mo μm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo ; A1 and A2 represent the sphericity of the first lithium iron phosphate material and the second lithium iron phosphate material respectively.

[0006] Some existing positive electrode active materials generally regulate the compaction density of positive electrode active materials by studying the particle size and particle size distribution of lithium iron phosphate materials, and rarely consider the contribution of particle sphericity in particle stacking. This means that when the compaction density of the mixed lithium iron phosphate positive electrode material increases, the charge and discharge cycle performance of its lithium ion battery will deteriorate. The lithium iron phosphate positive electrode active material provided in the embodiment of the present application, by limiting the D of the two lithium iron phosphate materials constituting it mo Scope, and related D mo The relationship between the sphericity A and the packing density of the positive electrode active material can be guaranteed to be high when the two lithium iron phosphate materials are mixed at random, and the compaction density of the positive electrode sheet is high, which can be 2.6g / cm 3 The above helps to improve the energy density of the battery made of the positive electrode active material. In addition, the electrochemical performance of the battery made of the positive electrode active material is relatively good, especially its cycle performance will not deteriorate.

[0007] In some embodiments of the present application, 0.5≤0.643D 1 mo +0.439A1≤2.29; further, 0.6≤0.643D 1 mo +0.439A1≤2.29.

[0008] In some embodiments of the present application, 0.42≤1.07D 2 mo +2.44A2-1.70D 2 mo ×A2≤1.89.

[0009] In the present application, D of the first lithium iron phosphate material 1 mo Value and D of the second lithium iron phosphate material 2 mo The values ​​can be obtained through their laser particle size distribution diagrams respectively. The test method can be found in GB / T19077-2016 / ISO 13320:2009 Particle size distribution laser diffraction method. The specific test instrument used is a laser particle size analyzer (such as Malvern 3000).

[0010] The above-mentioned sphericity A1 and A2 can be obtained by averaging the ratio of the longest side to the shortest side of multiple particles (generally with 400-800 particles) of the scanning electron microscope (SEM) photos of the first lithium iron phosphate material and the second lithium iron phosphate material. Specifically, A1 is the SEM photo of the first lithium iron phosphate material, and the longest side and the shortest side of each particle are measured using Image J software. The sphericity of each particle is defined as the ratio of the shortest side to the longest side, and the sphericity A1 of the first lithium iron phosphate material is the average of the sphericity of all particles in the SEM photo. The closer A1 and A2 are to 1, the more the material tends to be an ideal sphere.

[0011] In this application, D 1 mo <D 2 mo , D 1 mo The lithium ion diffusion path of the small lithium iron phosphate material is relatively small, which has a better electrical performance for the manufactured battery. 2 mo Large lithium iron phosphate materials are more conducive to improving the compaction density of positive electrode active materials. mo The particle size is within the above range, and combined with the relationship between them and the above sphericity A1, A2, it can be ensured that the two lithium iron phosphate materials can form a dense stack when mixed in any proportion, thereby improving the compaction density of the positive electrode sheet made of the obtained positive electrode active material without damaging the battery's cycle performance.

[0012] In some embodiments of the present application, the D 1 mo The value range can be: 0.32μm≤D 1 mo ≤2.45μm. Furthermore, D 1 mo The value range is: 0.40μm≤D 1 mo ≤2.45μm.

[0013] In some embodiments of the present application, the D 2 mo The value range can be: 1.2μm≤D 2 mo ≤5μm. Furthermore, D 2 mo The value range is: 1.25μm≤D 2 mo ≤4.95μm.

[0014] D 1mo , D 2 mo In the above range and D 1 mo <D 2 mo When the two lithium iron phosphate materials are used, they can better ensure both the high compaction density of the positive electrode sheet and the good electrochemical performance of the battery.

[0015] In the implementation mode of the present application, 0.5≤A1<1, 0.5≤A2<1. The sphericity of the two lithium iron phosphate materials is within the above range, which can better ensure that the compaction density of the positive electrode sheet is high. Further, in some embodiments, the value range of A1 can be: 0.51≤A1≤0.95. The value range of A2 can be: 0.51≤A2≤0.95. In the present application, the mixing mass ratio of the above-mentioned first lithium iron phosphate material and the second lithium iron phosphate material can be any ratio, which can ensure that the maximum compaction density of the positive electrode sheet made by the lithium iron phosphate positive active material is high and the battery cycle performance is good. In some embodiments of the present application, the mixing mass ratio of the first lithium iron phosphate material and the second lithium iron phosphate material can be in the range of 1: (0.25-3), and further can be in the range of 1: (0.25-2.5), for example, in the range of 1: (0.4-1.5). At this time, the positive electrode active material mixed with these two lithium iron phosphate materials can better ensure both the high compaction density of the electrode and the good cycle performance of the battery.

[0016] In the present application, the surfaces of the first lithium iron phosphate material and the second lithium iron phosphate material may have a carbon coating layer, which can be obtained by sequentially sand milling, spray drying and sintering a mixed slurry of a phosphorus source, an iron source, a lithium source and a carbon source. The present application does not limit the specific preparation method of the two lithium iron phosphate materials. The presence of the carbon coating layer can make the first and second lithium iron phosphate materials have good conductivity and less side reactions with the electrolyte. The positive electrode active material obtained by mixing the two has good conductivity and good battery cycle performance.

[0017] The lithium iron phosphate positive electrode active material provided in the first aspect of the present application is prepared by mixing two lithium iron phosphate materials that meet the particle size and sphericity parameter requirements in any proportion, and has a high compaction density. The battery made of the positive electrode active material can also have good cycle performance, rate performance, etc.

[0018] The second aspect of the present application provides a method for preparing a lithium iron phosphate positive electrode active material, comprising the following steps:

[0019] A first lithium iron phosphate material and a second lithium iron phosphate material are provided, wherein the particle size corresponding to the volume distribution percentage of the first lithium iron phosphate material reaching the maximum is D 1 moμm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, where 1≤D 2 mo ≤5, and D 1 mo <D 2 mo The sphericity of the first lithium iron phosphate material and the second lithium iron phosphate material are A1 and A2 respectively, and 0.49<0.643D 1 mo +0.439A1<2.3,0.41<1.07D 2 mo +2.44A2-1.70D 2 mo ×A2<1.9;

[0020] The first lithium iron phosphate material and the second lithium iron phosphate material are mixed to obtain a lithium iron phosphate positive electrode active material.

[0021] The preparation method of the lithium iron phosphate positive electrode active material can ensure that the compaction density of the obtained positive electrode active material is high by mixing two lithium iron phosphate materials that meet the specific particle size parameter requirements in any proportion. The battery made of the positive electrode active material can also have good cycle performance, rate performance, etc. The preparation method is simple in process, easy to operate, and suitable for large-scale production.

[0022] The third aspect of the present application provides a positive electrode plate, which contains the lithium iron phosphate positive electrode active material as described in the first aspect of the present application, or contains the lithium iron phosphate positive electrode active material prepared by the preparation method as described in the second aspect of the present application.

[0023] In the embodiment of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, and the positive electrode active material layer includes the above-mentioned lithium iron phosphate positive electrode active material, a binder and a conductive agent.

[0024] In the embodiment of the present application, the maximum compaction density of the positive electrode sheet is 2.6 g / cm 3 In some embodiments, the maximum compacted density is 2.65-2.8 g / cm 3 , further can be 2.67-2.75g / cm 3 It should be noted that the maximum compaction density of the positive electrode plate refers to the compaction density of the positive electrode plate corresponding to when the active material particles in the positive electrode plate are pressed until the particles are broken under a certain pressure.

[0025] The positive electrode material layer can be formed by coating a positive electrode slurry containing lithium iron phosphate positive electrode active material, a conductive agent, a binder and a solvent on the positive electrode current collector. Among them, the solvent can be one or more of N-methylpyrrolidone (NMP), acetone and dimethylacetamide (DMAC). The positive electrode current collector includes any one of aluminum foil, carbon-coated aluminum foil and perforated aluminum foil. Among them, the conductive agent includes but is not limited to one or more of carbon nanotubes, graphene, carbon black and carbon fiber. The binder includes but is not limited to one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyacrylate, polyacrylonitrile (PAN), sodium carboxymethyl cellulose (CMC) and sodium alginate.

[0026] A fourth aspect of the present application provides a lithium-ion battery, which includes the positive electrode sheet as described in the third aspect of the present application.

[0027] In the embodiment of the present application, the lithium-ion battery further includes a negative electrode plate, and an electrolyte and a separator located between the positive electrode plate and the negative electrode plate.

[0028] The lithium-ion battery using the above-mentioned positive electrode plate has high energy density and excellent cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The cycle performance curves of the soft-pack batteries of Examples 1-5 and Comparative Examples 1-2 of the present application are shown. DETAILED DESCRIPTION

[0030] Described below are exemplary embodiments of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.

[0031] The technical solution of the present application is described below in conjunction with a number of specific embodiments.

[0032] Example 1

[0033] A method for preparing a lithium iron phosphate positive electrode active material comprises the following steps:

[0034] The first lithium iron phosphate material LFP-1 is selected. When the volume distribution percentage of LFP-1 reaches the maximum, the corresponding particle size is 0.46 μm and the sphericity is 0.8, that is, D 1 mo is 0.46, A1 is 0.8, 0.643D 1 mo+0.439A1=0.65; select the second lithium iron phosphate material LFP-2, the volume distribution percentage of LFP-2 reaches the maximum when the corresponding particle size is 1.08μm, and the sphericity is 0.7, that is, D 2 mo is 1.08, A2 is 0.7, 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=1.58;

[0035] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 4:6 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0036] The positive electrode active material LFP-3 is prepared into a positive electrode sheet: the LFP-3 material is mixed with a conductive agent - carbon nanotubes, a binder (specifically polyvinylidene fluoride (PVDF)), and a solvent N-methyl ketone pyrrole (NMP) in a mass ratio of 100:3:2:60, and after mixing evenly, a positive electrode slurry is obtained; the positive electrode slurry is coated on both sides of a carbon-coated aluminum foil, and after drying, a surface density of 360 g / m 2 The maximum compaction density of the positive electrode sheet without particle crushing was tested. The maximum compaction density of the positive electrode sheet is 2.72g / cm 3 .

[0037] A preparation method for a lithium-ion soft-pack battery: providing a negative electrode plate, which is formed by coating a mixed slurry containing graphite: conductive agent (carbon black): binder (specifically SBR): water = 100:2:5:120 (mass ratio) on a copper foil, and then drying it; using the positive electrode plate made of the positive electrode active material LFP-3 in Example 1 as the positive electrode, using a polypropylene film as a separator, and a solution of ethylene carbonate (EC) containing 1.0 mol / L LiPF6: dimethyl carbonate (DMC) = 1:1 (volume ratio) as an electrolyte, and assembling to obtain a soft-pack battery.

[0038] Example 2

[0039] A method for preparing a lithium iron phosphate positive electrode active material, which is different from Example 1 in that: LFP-1 material and LFP-2 material are mixed in a mass ratio of 7:3.

[0040] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 2 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 2 was measured to be 2.68 g / cm 3 .

[0041] Example 3

[0042] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0043] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 2.41 μm (i.e., D 1 mo 2.41), sphericity A1 is 0.7, and 0.643D 1 mo +0.439A1=1.86; the second lithium iron phosphate material LFP-2 is selected, and the particle size corresponding to the maximum volume distribution percentage of LFP-2 is 4.36μm (i.e. D 2 mo is 4.36), sphericity A2 is 0.6, and 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=1.68;

[0044] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 8:2 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0045] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 3 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 3 was measured to be 2.65 g / cm 3 .

[0046] Example 4

[0047] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0048] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.46 μm (i.e., D 1 mo is 0.46), sphericity A1 is 0.8, and 0.643D 1 mo +0.439A1=0.65; the second lithium iron phosphate material LFP-2 is selected, and the corresponding particle size when its volume distribution percentage reaches the maximum is 3.45μm (i.e. D 2 mo 3.45), sphericity A2 is 0.7, 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=1.29;

[0049] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 5:5 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0050] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 4 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 4 was measured to be 2.70 g / cm 3 .

[0051] Example 5

[0052] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0053] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 1.32 μm (i.e., D 1 mo is 1.32), sphericity A1 is 0.7, and 0.643D 1 mo +0.439A1=1.16; the second lithium iron phosphate material LFP-2 is selected, and the corresponding particle size when the volume distribution percentage reaches the maximum is 2.31μm (i.e. D 2 mo 2.31), sphericity A2 is 0.6, and 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=1.58;

[0054] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 4:6 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0055] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 5 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 5 was measured to be 2.68 g / cm 3 .

[0056] Example 6

[0057] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0058] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 3.16 μm (i.e., D 1 mo is 3.16), sphericity A1 is 0.58, and 0.643D 1 mo+0.439A1=2.29; the second lithium iron phosphate material LFP-2 is selected, and the corresponding particle size when its volume distribution percentage reaches the maximum is 4.94μm (i.e. D 2 mo is 4.94), sphericity A2 is 0.57, 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=1.89;

[0059] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 3:7 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0060] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 6 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 6 was measured to be 2.68 g / cm 3 .

[0061] Example 7

[0062] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0063] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.32 μm (i.e., D 1 mo is 0.32), sphericity A1 is 0.9, and 0.643D 1 mo +0.439A1=0.60; the second lithium iron phosphate material LFP-2 is selected, and the corresponding particle size when its volume distribution percentage reaches the maximum is 3.96μm (i.e. D 2 mo is 3.96), sphericity A2 is 0.89, 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=0.42;

[0064] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 4:6 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0065] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 6 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 6 was measured to be 2.66 g / cm 3 .

[0066] In order to highlight the beneficial effects of the present application, the following comparative examples 1-5 are provided.

[0067] Comparative Example 1

[0068] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0069] Select the first lithium iron phosphate material LFP-1, its D 1 mo is 3.32μm, A1 is 0.8, but 0.643D 1 mo +0.439A1=2.49, which is not within the range (0.49, 2.3) required by this application; the second lithium iron phosphate material LFP-2 is selected, D 2 mo 3.98μm, A2 is 0.9, but 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=0.37, which is not within the range (0.41,1.9) required by this application;

[0070] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 1:1 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0071] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 1 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 1 was measured to be 2.65 g / cm 3 .

[0072] Comparative Example 2

[0073] A lithium iron phosphate positive electrode material, wherein the particle size corresponding to the maximum volume distribution percentage is 0.88 μm, and the sphericity A is 0.9.

[0074] Referring to the method described in Example 1, the positive electrode material is made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the soft pack battery is 2.53 g / cm 3 .

[0075] Comparative Example 3

[0076] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0077] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.31 μm (i.e., D 1 mo is 0.31), sphericity A1 is 0.6, but 0.643D 1 mo+0.439A1=0.46, which is not within the range of (0.49, 2.3) required by this application; the second lithium iron phosphate material LFP-2 is selected, and the corresponding particle size when its volume distribution percentage reaches the maximum is 5.36μm (i.e. D 2 mo is 5.36), sphericity A2 is 0.55, but 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=2.07, which is not within the range (0.41,1.9) required by this application;

[0078] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 5:5 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0079] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 3 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 3 was measured to be 2.63 g / cm 3 .

[0080] Comparative Example 4

[0081] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0082] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.52 μm (i.e., D 1 mo is 0.52), sphericity A1 is 0.6, and 0.643D 1 mo +0.439A1=0.60; the second lithium iron phosphate material LFP-2 is selected, and the corresponding particle size when its volume distribution percentage reaches the maximum is 4.23μm (i.e. D 1 mo is 4.23), sphericity A2 is 0.9, but 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=0.25, which is not within the range (0.41,1.9) required by this application;

[0083] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 2:8 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0084] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 4 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 4 was measured to be 2.64 g / cm 3 .

[0085] Comparative Example 5

[0086] A method for preparing a lithium iron phosphate positive electrode active material, comprising:

[0087] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.34 μm (i.e., D 1 mo 0.34), sphericity A1 is 0.8, 0.643D 1 mo +0.439A1=0.57; the second lithium iron phosphate material LFP-2 is selected, whose sphericity A2 is 0.85, and the corresponding particle size when its volume distribution percentage reaches the maximum is 0.65μm (i.e. D 2 mo is 0.65), which is not within the range of 1-5 μm required by this application, and 1.07D 2 mo +2.44A2-1.70D 2 mo ×A2=1.83, within the range of (0.41, 1.9) required by this application;

[0088] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 4:6 to obtain the lithium iron phosphate positive electrode active material LFP-3.

[0089] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 5 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 5 was measured to be 2.52 g / cm 3 .

[0090] In order to strongly support the beneficial effects of the present application, the soft-pack batteries of each embodiment and comparative example were subjected to cycle performance tests: each soft-pack battery was subjected to 0.5C / 0.5C charge-discharge cycle test at 25°C, with a voltage range of 2.0-3.8V. The cycle performance curves of the soft-pack batteries of embodiments 1-7 and comparative examples 1-5 are as follows: Figure 1 The data of the first cycle coulombic efficiency and capacity retention rate of the batteries of various embodiments and comparative examples are summarized in the following Table 1.

[0091] Table 1

[0092]

[0093]

[0094] Depend on Figure 1 As can be seen from Table 1, although the charge and discharge cycle performance of the battery in Comparative Example 2 is good, the maximum compaction density of the electrode sheet is low, which is not conducive to improving the energy density of the battery. When the two lithium iron phosphate materials are mixed by the method provided in the present application, the compaction density of the positive electrode sheet made of the obtained positive electrode active material is high, which can be 2.6g / cm 3 Above, some can reach 2.68-2.75g / cm 3 At the same time, the electrochemical performance of the battery is relatively excellent, the first discharge specific capacity is high, the first coulomb efficiency is high, and the cycle performance can match the cycle performance of the battery with low compaction density in Comparative Example 2 (Examples 1-7). However, the positive electrode active material obtained by mixing two raw materials that do not meet the specific requirements of this application (Comparative Examples 1, 3-5) has a very low compaction density of the pole piece, or even if the compaction density can sometimes reach 2.6g / cm 3 However, the battery's charge and discharge cycle stability is poor. In general, it cannot take into account both high electrode density and good cycle performance.

[0095] The above only expresses several exemplary embodiments of the present application, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present application. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, which all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be based on the attached claims.

Claims

1. A lithium iron phosphate positive electrode active material, characterized in that: The lithium iron phosphate positive electrode active material is prepared by mixing a first lithium iron phosphate material and a second lithium iron phosphate material in a mass ratio of 1:(0.25-3), and 0.49<0.643D 1 mo +0.439A1<2.3,0.41<1.07D 2 mo +2.44A2-1.70D 2 mo ×A2<1.9; Wherein, the particle size corresponding to the maximum volume distribution percentage of the first lithium iron phosphate material is D 1 mo μm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo ; A1 and A2 represent the sphericity of the first lithium iron phosphate material and the second lithium iron phosphate material respectively; 0.5≤A1<1, 0.5≤A2<1.

2. The lithium iron phosphate positive electrode active material according to claim 1, characterized in that The D 1 mo The value range is: 0.32≤D 1 mo ≤2.

45.

3. The lithium iron phosphate positive electrode active material according to claim 1, characterized in that The D 2 mo The value range is: 1.2≤D 2 mo ≤5.

4. A method for preparing a lithium iron phosphate positive electrode active material, characterized in that: The following steps are involved: A first lithium iron phosphate material and a second lithium iron phosphate material are provided, wherein the particle size corresponding to the volume distribution percentage of the first lithium iron phosphate material reaching the maximum is D 1 mo μm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo The sphericity of the first lithium iron phosphate material and the second lithium iron phosphate material are A1 and A2 respectively, 0.5≤A1<1, 0.5≤A2<1, and 0.49<0.643D 1 mo +0.439A1<2.3,0.41<1.07D 2 mo +2.44A2-1.70D 2 mo ×A2<1.9; The first lithium iron phosphate material and the second lithium iron phosphate material are mixed in a mass ratio of 1:(0.25-3) to obtain a lithium iron phosphate positive electrode active material.

5. A positive electrode sheet, characterized in that: The positive electrode sheet contains the lithium iron phosphate positive electrode active material according to any one of claims 1 to 3 or includes the lithium iron phosphate positive electrode active material prepared by the preparation method according to claim 4.

6. The positive electrode sheet according to claim 5, characterized in that: The maximum compaction density of the positive electrode sheet is 2.6 g / cm 3 above.

7. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 5 or 6.

Citation Information

Patent Citations

  • Active material, battery, and method for manufacturing electrode

    CN101882679A

  • Electrode, secondary battery, battery pack, electric vehicle and electric power storage system

    CN103165935A

  • Positive electrode material for battery, battery positive electrode, battery and preparation method of positive electrode material

    CN111162258A

  • Positive electrode material, and electrochemical device and electronic device comprising same

    CN113169322A

  • Electrochemical device and electronic device including same

    CN114041226A