A lithium iron phosphate positive electrode active material and preparation method thereof, positive electrode sheet and lithium ion battery
By regulating the particle size and particle size distribution of the lithium iron phosphate material, the mixed cathode active material improves the compaction density and electrochemical performance of the battery, solves the problem of low energy density of the lithium iron phosphate material, and achieves high energy density and excellent Taking into account cycle performance.
Patent Information
- Application Number
- CN202210228274.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-03-07
AI Technical Summary
The maximum compacted density of lithium iron phosphate cathode material is small, resulting in a low energy density of the battery, which cannot meet the market demand for high endurance. At the same time, increasing the compacted density will damage the electrochemical performance of the battery.
By regulating the particle size parameters of the two lithium iron phosphate materials, the mixed cathode active material can achieve high compaction density while maintaining excellent electrochemical performance. The specific method is to limit the particle size of the first and second lithium iron phosphate materials. The diameter range and particle size distribution dispersion range, combined with the test of laser particle size distribution chart, ensure that the compacted density of the mixture is above 2.6g/cm3.
The high compaction density and good cycle performance of the positive electrode sheet are achieved, and the energy density and electrochemical performance of the battery, especially the cycle performance, are improved.
Smart Images

Figure CN116779842B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium-ion batteries, and in particular to a lithium iron phosphate positive electrode active material and a preparation method thereof, a positive electrode sheet and a lithium-ion battery. Background Art
[0002] Lithium iron phosphate materials are widely used due to their advantages such as high safety, low price and environmental friendliness. However, lithium iron phosphate cathode materials have an obvious disadvantage, that is, their maximum compaction density is relatively small (2.1-2.5g / cm 3 ), resulting in low energy density of batteries made from it, which cannot meet the market demand for batteries with long battery life. In order to improve the energy density of batteries, high-density lithium iron phosphate materials are the mainstream development direction in the industry, but while increasing their compaction density, the electrochemical performance of the battery is often reduced. Summary of the invention
[0003] In view of this, the present application provides a lithium iron phosphate positive electrode active material and a preparation method thereof, a positive electrode plate and a lithium ion battery. By regulating the particle size parameters of the two lithium iron phosphate materials that constitute it, the compaction density of the positive electrode active material mixed in any proportion can be high, and the electrochemical performance of the battery is relatively good.
[0004] Specifically, in the first aspect, the present application provides a lithium iron phosphate positive electrode active material, which is formed by mixing a first lithium iron phosphate material and a second lithium iron phosphate material; wherein the particle size corresponding to the volume distribution percentage of the first lithium iron phosphate material reaching the maximum is D 1 mo μm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo The particle size distribution dispersion of the first lithium iron phosphate material is A1, and the particle size distribution dispersion of the second lithium iron phosphate material is A2, 1≤A1≤3, 2≤A2≤4; and 4.07<A1×(2.31+D 1 mo )<16,-0.4<A2×(D 2 mo -1.15)<14.
[0005] The lithium iron phosphate positive electrode active material provided in the embodiment of the present application is provided by defining the D of the two lithium iron phosphate materials constituting the lithium iron phosphate positive electrode active material.mo Range, range of particle size distribution dispersion A, and related D mo The relationship range with A can ensure that the compaction density of the positive electrode sheet made of the positive electrode active material mixed with these two lithium iron phosphate materials in any proportion is high, which can be 2.6g / cm 3 The above helps to improve the energy density of the battery made of the positive electrode active material. In addition, the electrochemical performance of the battery made of the positive electrode active material is also relatively good, especially its cycle performance. In some embodiments of the present application, 4.08≤A1×(2.31+D 1 mo )≤15.9; preferably, A1×(2.31+D 1 mo ) can be in the range of 4.11-15.86.
[0006] In some implementations of the present application, -0.38≤A2×(D 2 mo -1.15)≤13.95.
[0007] In the present application, D of the first lithium iron phosphate material 1 mo Value and D of the second lithium iron phosphate material 2 mo The values can be obtained through their laser particle size distribution diagrams respectively. The specific testing instrument is a laser particle size analyzer (such as Malvern 3000). The testing method can be found in GB / T 19077-2016 / ISO 13320:2009 Particle size distribution laser diffraction method.
[0008] The particle size distribution dispersion of the first lithium iron phosphate material is A1=(D 1 90 -D 1 10 ) / D 1 50 , the particle size distribution dispersion of the second lithium iron phosphate material A2=(D 2 90 -D 2 10 ) / D 2 50 Among them, D 1 90 The particle size value corresponding to the volume cumulative distribution percentage reaching 90% in the laser particle size distribution diagram of the first lithium iron phosphate material; D 1 10 represents the particle size value corresponding to when the volume cumulative distribution percentage of the first lithium iron phosphate material reaches 10%; D 1 50represents the particle size value corresponding to when the volume cumulative distribution percentage of the first lithium iron phosphate material reaches 50%. The smaller the A1 value is, the smaller the particle size distribution dispersion of the first lithium iron phosphate material is (or the narrower the particle size distribution width is), and the higher the particle size distribution concentration is. Similarly, D 2 90 , D 2 10 , D 2 50 They represent the particle size values corresponding to the volume cumulative distribution percentages reaching 90%, 10%, and 50% in the laser particle size distribution diagram of the second lithium iron phosphate material. 2 90 , D 2 10 , D 2 50 Value and D of the second lithium iron phosphate material 2 90 , D 2 10 , D 2 50 The values can also be obtained through their laser particle size distribution diagrams. The test methods can be found in GB / T 19077-2016 / ISO 13320:2009 Particle size distribution laser diffraction method.
[0009] In this application, D 1 mo <D 2 mo , D 1 mo The lithium ion diffusion path of the small lithium iron phosphate material is relatively small, which has a better electrical performance for the manufactured battery. 2 mo Large lithium iron phosphate materials are more conducive to improving the compaction density of positive electrode active materials. mo The particle size is within the above range, and combined with the above ranges of A1 and A2 and the relationship between them, it can be ensured that the two lithium iron phosphate materials can form a dense stack when mixed in any proportion, thereby improving the compaction density of the positive electrode sheet made from the obtained positive electrode active material without damaging the cycle performance of the battery.
[0010] In some embodiments of the present application, the D 1 mo The value range of can be: 0.31≤D 1 mo ≤2.5. Furthermore, D 1 mo The value range is: 0.35≤D 1 mo ≤2.46.
[0011] In some embodiments of the present application, the D 2 mo The value range of can be: 1.2≤D 2 mo ≤5. Furthermore, D 2 mo The value range is: 1.2≤D 2 mo ≤4.5; further, D 2 mo The value range is: 1.25≤D 2 mo ≤4.48.
[0012] D 1 mo , D 2 mo In the above range and satisfying D 1 mo <D 2 mo When the two lithium iron phosphate materials are used, they can better ensure both the high compaction density of the positive electrode sheet and the good electrochemical performance of the battery.
[0013] In the present application, the mixing mass ratio of the first lithium iron phosphate material and the second lithium iron phosphate material can be any ratio, which can ensure that the maximum compaction density of the positive electrode sheet made by the lithium iron phosphate positive electrode active material is high and the battery cycle performance is good. In some embodiments of the present application, the mixing mass ratio of the first lithium iron phosphate material and the second lithium iron phosphate material can be in the range of 1: (0.4-4), and further in the range of 1: (0.6-2.5), for example, in the range of 1: (1-2.5). At this time, the positive electrode active material mixed with these two lithium iron phosphate materials can better ensure both the high compaction density of the electrode sheet and the good cycle performance of the battery.
[0014] In the present application, the surfaces of the first lithium iron phosphate material and the second lithium iron phosphate material may have a carbon coating layer, which can be obtained by sequentially sand milling, spray drying and sintering a mixed slurry of a phosphorus source, an iron source, a lithium source and a carbon source. The present application does not limit the specific preparation method of the two lithium iron phosphate materials. The presence of the carbon coating layer can make the first and second lithium iron phosphate materials have good conductivity and less side reactions with the electrolyte. The positive electrode active material obtained by mixing the two has good conductivity and good battery cycle performance.
[0015] The lithium iron phosphate positive electrode active material provided in the first aspect of the present application is formed by mixing two lithium iron phosphate materials that meet specific particle size parameter requirements in any proportion. The positive electrode sheet made of the positive electrode active material has a high compaction density, and the battery can also have good cycle performance, rate performance, etc.
[0016] The second aspect of the present application provides a method for preparing a lithium iron phosphate positive electrode active material, comprising the following steps:
[0017] A first lithium iron phosphate material and a second lithium iron phosphate material are provided, wherein the particle size corresponding to the volume distribution percentage of the first lithium iron phosphate material reaching the maximum is D 1 mo μm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo The particle size distribution dispersion of the first lithium iron phosphate material is A1, and the particle size distribution dispersion of the second lithium iron phosphate material is A2, wherein 1≤A1≤3, 2≤A2≤4, and 4.07<A1×(2.31+D 1 mo )<16,-0.4<A2×(D 2 mo -1.15)<14.
[0018] The first lithium iron phosphate material and the second lithium iron phosphate material are mixed to obtain a lithium iron phosphate positive electrode active material.
[0019] The preparation method of the lithium iron phosphate positive electrode active material can ensure that the compaction density of the obtained positive electrode active material is high by mixing two lithium iron phosphate materials that meet the specific particle size parameter requirements in any proportion. The battery made of the positive electrode active material can also have good cycle performance, rate performance, etc. The preparation method is simple in process, easy to operate, and suitable for large-scale production.
[0020] The third aspect of the present application provides a positive electrode plate, which contains the lithium iron phosphate positive electrode active material as described in the first aspect of the present application, or contains the lithium iron phosphate positive electrode active material prepared by the preparation method as described in the second aspect of the present application.
[0021] In the embodiment of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer arranged on the surface of the positive electrode current collector, and the positive electrode active material layer includes the above-mentioned lithium iron phosphate positive electrode active material, a binder and a conductive agent.
[0022] In the embodiment of the present application, the maximum compaction density of the positive electrode sheet is 2.6 g / cm 3In some embodiments, the maximum compacted density is 2.62-2.8 g / cm 3 , further can be 2.65-2.75g / cm 3 It should be noted that the maximum compaction density of the positive electrode plate refers to the compaction density of the plate corresponding to when the active material particles in the positive electrode plate are pressed to pieces under a certain pressure.
[0023] The positive electrode material layer can be formed by coating a positive electrode slurry containing lithium iron phosphate positive electrode active material, a conductive agent, a binder and a solvent on the positive electrode current collector. Among them, the solvent can be one or more of N-methylpyrrolidone (NMP), acetone and dimethylacetamide (DMAC). The positive electrode current collector includes any one of aluminum foil, carbon-coated aluminum foil and perforated aluminum foil. Among them, the conductive agent includes but is not limited to one or more of carbon nanotubes, graphene, carbon black and carbon fiber. The binder includes but is not limited to one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyacrylate, polyacrylonitrile (PAN), sodium carboxymethyl cellulose (CMC) and sodium alginate.
[0024] A fourth aspect of the present application provides a lithium-ion battery, which includes the positive electrode sheet as described in the third aspect of the present application.
[0025] In the embodiment of the present application, the lithium-ion battery further includes a negative electrode plate, and an electrolyte and a separator located between the positive electrode plate and the negative electrode plate.
[0026] The lithium-ion battery using the above-mentioned positive electrode plate has high energy density and excellent cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The cycle performance curves of the soft-pack batteries of Examples 1-5 and Comparative Examples 1-2 of the present application are shown. DETAILED DESCRIPTION
[0028] Described below are exemplary embodiments of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.
[0029] The technical solution of the present application is described below in conjunction with a number of specific embodiments.
[0030] Example 1
[0031] A method for preparing a lithium iron phosphate positive electrode active material comprises the following steps:
[0032] The first lithium iron phosphate material LFP-1 is selected. When the volume distribution percentage of LFP-1 reaches the maximum, the corresponding particle size is 0.31 μm, and the particle size distribution dispersion is 2.22, that is, D 1 mo is 0.31, A1 is 2.22, and A1×(2.31+D 1 mo )=5.82; Select the second lithium iron phosphate material LFP-2, the volume distribution percentage of LFP-2 reaches the maximum when the corresponding particle size is 1.28μm, and the particle size distribution dispersion is 2.24, that is, D 2 mo is 1.28, A2 is 2.24, and A2×(D 2 mo -1.15)=0.29;
[0033] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 2:8 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0034] The positive electrode active material LFP-3 is prepared into a positive electrode sheet: the LFP-3 material is mixed with a conductive agent - carbon nanotubes, a binder (specifically polyvinylidene fluoride (PVDF)), and a solvent N-methyl ketone pyrrole (NMP) in a mass ratio of 100:3:2:60, and after mixing evenly, a positive electrode slurry is obtained; the positive electrode slurry is coated on both sides of a carbon-coated aluminum foil, and after drying, a surface density of 360 g / m 2 The maximum compaction density of the positive electrode sheet without particle crushing was tested. The maximum compaction density of the positive electrode sheet is 2.70g / cm 3 .
[0035] A preparation method for a lithium-ion soft-pack battery: providing a negative electrode plate, which is formed by coating a mixed slurry containing graphite: conductive agent (carbon black): binder (specifically SBR): water = 100:2:5:120 (mass ratio) on a copper foil, and then drying it; using the positive electrode plate made of the positive electrode active material LFP-3 in Example 1 as the positive electrode, using a polypropylene film as a separator, and a solution of ethylene carbonate (EC) containing 1.0 mol / L LiPF6: dimethyl carbonate (DMC) = 1:1 (volume ratio) as an electrolyte, and assembling to obtain a soft-pack battery.
[0036] Example 2
[0037] A method for preparing a lithium iron phosphate positive electrode active material, which is different from Example 1 in that: LFP-1 material and LFP-2 material are mixed in a mass ratio of 4:6.
[0038] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 2 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 2 was measured to be 2.68 g / cm 3 .
[0039] Example 3
[0040] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0041] The first lithium iron phosphate material LFP-1 is selected. When the volume distribution percentage of LFP-1 reaches the maximum, the corresponding particle size is 3.12 μm, and the particle size distribution dispersion is 2.92, that is, D 1 mo is 3.12, A1 is 2.92, and A1×(2.31+D 1 mo )=15.86; Select the second lithium iron phosphate material LFP-2, the volume distribution percentage of LFP-2 reaches the maximum when the corresponding particle size is 4.93μm, and the particle size distribution dispersion is 3.69, that is, D 2 mo is 4.93, A2 is 3.69, and A2×(D 2 mo -1.15)=13.95;
[0042] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 5:5 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0043] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 4 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 4 was measured to be 2.73 g / cm 3 .
[0044] Example 4
[0045] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0046] The first lithium iron phosphate material LFP-1 is selected. When the volume distribution percentage of LFP-1 reaches the maximum, the corresponding particle size is 1.41 μm, and the particle size distribution dispersion is 2.32, that is, D 1 mo is 1.41, A1 is 2.32, and A1×(2.31+D 1 mo )=8.63; Select the second lithium iron phosphate material LFP-2, the volume distribution percentage of LFP-2 reaches the maximum when the corresponding particle size is 3.36μm, and the particle size distribution dispersion is 2.58, that is, D 2mo is 3.36, A2 is 2.58, and A2×(D 2 mo -1.15)=5.70;
[0047] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 3:7 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0048] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 3 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 3 was measured to be 2.68 g / cm 3 .
[0049] Example 5
[0050] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0051] The first lithium iron phosphate material LFP-1 is selected. When the volume distribution percentage reaches the maximum, the corresponding particle size is 2.46 μm, and the particle size distribution dispersion is 2.16, that is, D 1 mo is 2.46, A1 is 2.16, and A1×(2.31+D 1 mo )=10.30; select the second lithium iron phosphate material LFP-2, the volume distribution percentage of which reaches the maximum when the corresponding particle size is 4.48μm, the particle size distribution dispersion is 3.92, that is, D 2 mo is 4.48 μm, A2 is 3.92, and A2×(D 2 mo -1.15)=13.05;
[0052] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 7:3 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0053] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 5 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 5 was measured to be 2.65 g / cm 3 .
[0054] Example 6
[0055] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0056] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.8 μm, and the particle size distribution dispersion is 1.32, that is, D 1mo is 0.8, A1 is 1.32, and A1×(2.31+D 1 mo )=4.11;Select the second lithium iron phosphate material LFP-2, the volume distribution percentage of which reaches the maximum when the corresponding particle size is 1.65μm, and the particle size distribution dispersion is 3.6, that is, D 2 mo is 1.65, A2 is 3.6, and A2×(D 2 mo -1.15)=1.8;
[0057] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 3:7 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0058] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Example 6 was made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the positive electrode sheet of Example 6 was measured to be 2.66 g / cm 3 .
[0059] Example 7
[0060] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0061] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.64 μm, and the particle size distribution dispersion is 2.8, that is, D 1 mo is 0.64, A1 is 2.8, and A1×(2.31+D 1 mo )=8.26; Select the second lithium iron phosphate material LFP-2, the volume distribution percentage of which reaches the maximum when the corresponding particle size is 1.02μm, the particle size distribution dispersion is 2.94, that is, D 2 mo is 1.02, A2 is 2.94, and A2×(D 2 mo -1.15) = -0.38;
[0062] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 6:4 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0063] The positive electrode active material LFP-3 obtained in Example 7 was made into a positive electrode sheet according to the method described in Example 1, and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Example 7 was measured to be 2.65 g / cm 3 .
[0064] In order to highlight the beneficial effects of the present application, the following comparative examples 1-6 are provided.
[0065] Comparative Example 1
[0066] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0067] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.35 μm (ie, D 1 mo is 0.35), the particle size distribution dispersion A1 is 1.27, but A1×(2.31+D 1 mo )=3.38, which is not within the range of (4.07,16) required by the present application; the second lithium iron phosphate material LFP-2 is selected, and the particle size corresponding to the maximum volume distribution percentage is 1.03 μm (i.e., D 2 mo is 1.03), the particle size distribution dispersion A2 is 3.87, but A2×(D 2 mo -1.15) = -0.46, which is not within the range of (-0.4, 14) required by this application;
[0068] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 1:1 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0069] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 1 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 1 was measured to be 2.58 g / cm 3 .
[0070] Comparative Example 2
[0071] A lithium iron phosphate positive electrode material, wherein the particle size corresponding to the maximum volume distribution percentage is 0.31 μm, and the particle size distribution dispersion A is 1.92.
[0072] Referring to the method described in Example 1, the positive electrode material is made into a positive electrode sheet and assembled into a soft pack battery. The maximum compaction density of the soft pack battery is 2.55 g / cm 3 .
[0073] Comparative Example 3
[0074] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0075] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.35 μm (i.e., D 1 mois 0.35), the particle size distribution dispersion A1 is 1.24, but A1×(2.31+D 1 mo )=3.30, which is not within the range of (4.07,16) required by the present application; the second lithium iron phosphate material LFP-2 is selected, and the particle size corresponding to the maximum volume distribution percentage is 5.11 μm (i.e., D 2 mo is 5.11), which is not within the range of (1,5) required by this application. The particle size distribution dispersion A2 is 3.78, and A2×(D 2 mo -1.15) = 14.97, which is not within the range of (-0.4, 14) required by this application;
[0076] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 2:8 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0077] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 3 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 3 was measured to be 2.63 g / cm 3 .
[0078] Comparative Example 4
[0079] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0080] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.46 μm (ie, D 1 mo is 0.46), the particle size distribution dispersion A1 is 1.22, but A1×(2.31+D 1 mo )=3.38, which is not within the range of (4.07,16) required by the present application; the second lithium iron phosphate material LFP-2 is selected, and the particle size corresponding to the maximum volume distribution percentage is 1.47 μm (i.e., D 2 mo is 1.47), the particle size distribution dispersion A2 is 2.66, A2×(D 2 mo -1.15)=0.85, within the range of (-0.4,14) required by this application;
[0081] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 3:7 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0082] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 4 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 4 was measured to be only 2.57 g / cm 3 .
[0083] Comparative Example 5
[0084] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0085] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 3.1 μm (ie, D 1 mo is 3.1), and within the range of 0.3-3.2 μm required in this application, the particle size distribution dispersion A1 is 2.58, A1×(2.31+D 1 mo )=13.96;Select the second lithium iron phosphate material LFP-2, the volume distribution percentage of which reaches the maximum when the corresponding particle size is 5.23μm (ie, D 2 mo is 5.23), which is not within the range of (1,5) required by this application. The particle size distribution dispersion A2 is 3.29, A2×(D 2 mo -1.15)=13.42, within the range of (-0.4,14) required by this application;
[0086] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 5:5 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0087] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 5 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 5 was measured to be 2.62 g / cm 3 .
[0088] Comparative Example 6
[0089] A method for preparing a lithium iron phosphate positive electrode active material, comprising:
[0090] The first lithium iron phosphate material LFP-1 is selected, and the particle size corresponding to the maximum volume distribution percentage is 0.54 μm (ie, D 1 mo is 0.54), the particle size distribution dispersion A1 is 1.87, A1×(2.31+D 1 mo )=5.33; select the second lithium iron phosphate material LFP-2, the volume distribution percentage of which reaches the maximum when the corresponding particle size is 1.12μm (ie, D 2mo is 1.12), the particle size distribution dispersion A2 is 1.61, which is not within the range of 2-4 required by this application, A2×(D 2 mo-1.15)=-0.05;
[0091] The LFP-1 material and the LFP-2 material were mixed in a mass ratio of 6:4 to obtain the lithium iron phosphate positive electrode active material LFP-3.
[0092] Referring to the method described in Example 1, the positive electrode active material LFP-3 obtained in Comparative Example 6 was made into a positive electrode sheet and assembled into a soft-pack battery. The maximum compaction density of the positive electrode sheet of Comparative Example 6 was measured to be 2.54 g / cm 3 .
[0093] In order to strongly support the beneficial effects of the present application, the soft-pack batteries of each embodiment and comparative example were subjected to cycle performance tests: 0.5C / 0.5C charge-discharge cycle tests were performed on each soft-pack battery at 25°C, with a voltage range of 2.0-3.8V. The cycle performance curves of the soft-pack batteries of embodiments 1-5 and comparative examples 1-2 are as follows: Figure 1 The data of the first cycle coulombic efficiency and capacity retention rate of the batteries of various embodiments and comparative examples are summarized in the following Table 1.
[0094] Table 1
[0095]
[0096]
[0097] Depend on Figure 1 As can be seen from Table 1, although the charge and discharge cycle performance of the battery in Comparative Example 2 is good, the maximum compaction density of the electrode sheet is low, which is not conducive to improving the energy density of the battery. When the two lithium iron phosphate materials are mixed by the method provided in the present application, the compaction density of the positive electrode sheet made of the obtained positive electrode active material is high, which can be 2.6g / cm 3 Above, some can reach 2.65-2.75g / cm 3 At the same time, the electrochemical performance of the battery is relatively excellent, the first discharge specific capacity is high, the first coulomb efficiency is high, and the cycle performance can match the cycle performance of the battery with low compaction density in Comparative Example 2 (Examples 1-7). However, the positive electrode active material obtained by mixing two raw materials that do not meet the specific requirements of this application (Comparative Examples 1, 3-6) has a very low compaction density of the pole piece, or even if the compaction density can sometimes reach 2.6g / cm 3 However, the battery's charge and discharge cycle stability is poor. In general, it cannot take into account both high electrode density and good cycle performance.
[0098] The above only expresses several exemplary embodiments of the present application, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present application. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present application, which all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be based on the attached claims.
Claims
1. A lithium iron phosphate positive electrode active material, characterized in that: The lithium iron phosphate positive electrode active material is formed by mixing a first lithium iron phosphate material and a second lithium iron phosphate material; Wherein, the particle size corresponding to the maximum volume distribution percentage of the first lithium iron phosphate material is D 1 mo μm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo ; The particle size distribution dispersion of the first lithium iron phosphate material is A1, and the particle size distribution dispersion of the second lithium iron phosphate material is A2, wherein 1≤A1≤3, 2≤A2≤4, And 4.07<A1×(2.31+D 1 mo )<16,-0.4<A2×(D 2 mo -1.15)<14.
2. The lithium iron phosphate positive electrode active material according to claim 1, characterized in that The D 1 mo The value range is: 0.31≤D 1 mo ≤2.
5.
3. The lithium iron phosphate positive electrode active material according to claim 1, characterized in that The D 2 mo The value range is: 1.2≤D 2 mo ≤4.
5.
4. The lithium iron phosphate positive electrode active material according to claim 1, characterized in that The mixing mass ratio of the first lithium iron phosphate material to the second lithium iron phosphate material is in the range of 1:(0.4-4).
5. The lithium iron phosphate positive electrode active material according to any one of claims 1 to 4, characterized in that: The surfaces of the first lithium iron phosphate material and the second lithium iron phosphate material have a carbon coating layer.
6. A method for preparing a lithium iron phosphate positive electrode active material, characterized in that: The following steps are involved: A first lithium iron phosphate material and a second lithium iron phosphate material are provided, wherein the particle size corresponding to the volume distribution percentage of the first lithium iron phosphate material reaching the maximum is D 1 mo μm, 0.3≤D 1 mo ≤3.2, the particle size corresponding to the volume distribution percentage of the second lithium iron phosphate material reaching the maximum is D 2 mo μm, 1≤D 2 mo ≤5, and D 1 mo <D 2 mo The particle size distribution dispersion of the first lithium iron phosphate material is A1, the particle size distribution dispersion of the second lithium iron phosphate material is A2, 1≤A1≤3, 2≤A2≤4, and 4.07<A1×(2.31+D 1 mo )<16,-0.4<A2×(D 2 mo -1.15)<14; The first lithium iron phosphate material and the second lithium iron phosphate material are mixed to obtain a lithium iron phosphate positive electrode active material.
7. A positive electrode sheet, characterized in that: The positive electrode sheet contains the lithium iron phosphate positive electrode active material according to any one of claims 1 to 5 or includes the lithium iron phosphate positive electrode active material prepared by the preparation method according to claim 6.
8. The positive electrode sheet according to claim 7, characterized in that: The maximum compaction density of the positive electrode sheet is 2.6 g / cm 3 above.
9. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet according to claim 7 or 8.
Citation Information
Cited By
Lithium iron phosphate positive electrode active material, preparation method therefor, and lithium ion battery
EP4481856A1