A method for preparing droplet sample by microwave curing process

By separating carbon fibers and resin from the prepreg, embedded in auxiliary vehicles and preparing droplet samples by microwave heating, the problem of fiber and resin droplet samples preparation in the prior art was solved, and fibers in the microwave curing process were realized The effective characterization of the interface with resin has improved the research on the mechanical properties of composite materials.

CN116793792BActive Publication Date: 2024-11-08CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310779178.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-29
Publication Date
2024-11-08
Estimated Expiration
2043-06-29

AI Technical Summary

Technical Problem

The existing micro droplet preparation methods are not suitable for preparing micro droplet samples of fibers and resins to characterize the interfacial bonding performance between fibers and resins in microwave curing processes, which affects the study of the mechanical properties of composite materials.

Method used

Separate the dry carbon fiber bundle from the prepreg, embed it into the auxiliary vehicle and set the weight to generate preload force, apply the resin evenly, prepare the droplet sample using microwave heating process, control the temperature and heating rate to ensure the fiber and resin effective combination.

Benefits of technology

The simplicity of the preparation method and the controllability of the droplet size are achieved, and the mechanical behavior and damage mechanism of the fiber and resin interface in the microwave curing process can be evaluated more closely to the actual working conditions, which has important economic value and theoretical research significance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116793792B_ABST
    Figure CN116793792B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a droplet sample by using a microwave curing process, comprising the following steps: S1, taking out a plurality of fiber filaments from a fiber bundle separated from a prepreg and dried, and embedding the fiber filaments into a fiber filament placement groove; S2, setting weights at both ends of the fiber filaments to produce a pre-tightening force for straightening the fiber filaments; S3, taking out an appropriate amount of resin, smearing it on the fiber filaments above the resin holding groove, and letting it stand in an auxiliary carrier for a period of time; S4, microwave heating the finally obtained droplet sample. The preparation method of the droplet sample for microwave curing process of the present invention is used to characterize the fiber-resin interface bonding strength of the microwave curing process. The preparation method is simple, the droplet size is controllable, and the evaluation method is closer to the actual working condition. It has important economic value and theoretical research significance, and is also the focus and hotspot of research in this field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microdroplet preparation, and in particular to a method for preparing a microdroplet sample by adopting a microwave curing process. Background Art

[0002] Carbon fiber reinforced resin-based composite materials are widely used in aerospace, transportation, medical, sports building materials and other fields due to their high specific strength, high specific stiffness, fatigue resistance, and designable material properties. Microwave curing process is one of the composite tank curing molding processes. Due to its unique "in-volume" heating method, it has the characteristics of high energy utilization, fast heating speed, uniform temperature distribution of parts, easy temperature control during molding, and high resin and fiber bonding strength. It has attracted extensive attention from researchers. Among them, the improvement of the fiber and resin interface bonding strength is crucial to the improvement of the overall mechanical properties of composite materials. The droplet debonding method is a method to characterize the interface bonding strength between fiber and resin. At the same time, because the carbon fiber composite material is prepreg, which is a mixture of fiber and resin, in order to prepare the droplet debonding specimen, the fiber and resin must be separated first, and then the microwave curing process is used to prepare the specimen, so that the bonding performance of the interface between fiber and resin in the microwave curing process can be identified and characterized, and the mechanical behavior and failure mechanism of the fiber and resin interface in the microwave curing process can be revealed. It has important economic value and theoretical research significance, and is also the focus and hot spot of research in this field.

[0003] In the prior art, for example, the invention patent application with application number 201910828457.4 discloses a droplet preparation system and preparation method, which includes the following steps: configuring a sample on a microfluidic chip; clamping the microfluidic chip, and connecting the gas circuit module to the gas source; the gas source inputs gas into the gas circuit module, and the gas flows to each continuous phase inlet and each dispersed phase inlet through the gas circuit module for a duration of T; after the droplet preparation is completed, the microfluidic chip is taken out. When preparing droplets, the gas applies air pressure to the continuous phase inlet and the dispersed phase inlet respectively through the gas circuit module, so that the continuous phase in the continuous phase inlet and the dispersed phase in the dispersed phase inlet flow to the corresponding droplet outlet to achieve the preparation of droplets, and the operation process is simple. The existing droplet preparation method is to inject an immiscible liquid into a microfluidic chip and prepare uniform droplets that meet various size requirements at an extremely fast speed, but this method is not suitable for the preparation of droplet samples using fibers and resins to characterize the bonding performance of the interface between fibers and resins in microwave curing processes. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a droplet sample by using a microwave curing process to solve the problems raised in the background technology.

[0005] To achieve the above object, the present invention provides a method for preparing a droplet sample by using a microwave curing process, comprising the following steps:

[0006] S1, taking out a plurality of fiber filaments from the carbon fiber bundle separated from the prepreg and dried, and embedding the plurality of fiber filaments one by one into a plurality of fiber filament placement grooves of the auxiliary carrier;

[0007] S2. Set 2-5g weights at both ends of each fiber to produce a pre-tightening force to straighten the fiber;

[0008] S3, taking out a proper amount of resin with a needle, and evenly applying it on the surface of the fiber filament above the resin holding tank, and controlling the diameter of the droplet to be between 30 and 50 microns, and then leaving the fiber filament after application in the auxiliary carrier for 30 to 50 minutes;

[0009] S4. Place the auxiliary carrier embedded with the fiber filaments as a whole into a heating furnace with a microwave generator, and suspend the weight in the air. Turn on the microwave heating furnace to heat the droplet sample in the auxiliary carrier from room temperature to 125-135°C, keep it warm for a period of time and then stop heating. Then cool it as the microwave heating furnace, take out the cooled auxiliary carrier from the microwave heating furnace, loosen the weight, and take out the droplet sample in the auxiliary carrier.

[0010] Furthermore, the droplet sample in the auxiliary carrier is heated from room temperature to 125-135° C. at a heating rate of 1.5-3° C. / min, and the heating is stopped after being kept at this temperature for 120-135 min.

[0011] Furthermore, the auxiliary carrier includes a carrier body, and a plurality of parallel and spaced fiber filament insertion grooves are provided on the surface of the carrier body, and a resin receiving groove is provided at the center of each of the fiber filament insertion grooves, and the fiber filament insertion grooves and the resin receiving grooves are both recessed inward from the surface of the carrier body.

[0012] Furthermore, the method of the present invention further comprises the step of separating fibers from the prepreg before step S1:

[0013] S01, taking out the prepreg from the low temperature environment and thawing it, and cutting the thawed prepreg into a plurality of prepreg sheets;

[0014] S02, tear off the protective stickers on the surfaces of the cut prepreg sheets, and put all the prepreg sheets into a dissolving container in the same fiber direction, pour an appropriate amount of acetone solution into the dissolving container, and let the prepreg sheets stand and dissolve in the acetone solution for a period of time; repeat the dissolution 4 to 6 times, and collect the mixed solution of acetone and resin matrix in a beaker after each dissolution;

[0015] S03, placing the dissolved fiber into an ultrasonic cleaner, and pouring an appropriate amount of anhydrous ethanol solution into it, ultrasonically cleaning the acetone and resin matrix mixed solution remaining on the surface of the carbon fiber, repeating the cleaning 2 to 3 times, each cleaning time is 4 to 10 minutes;

[0016] S04, the carbon fibers after ultrasonic cleaning are bundled together with pressure-sensitive tape in the same fiber direction, and placed in an autoclave, the autoclave is heated to 120-150°C at a heating rate of 1-5°C / min, and the temperature is maintained at a constant temperature for 2-3h, and then naturally cooled to room temperature to obtain a dry carbon fiber bundle;

[0017] S05, placing the beaker containing the acetone and resin matrix mixed solution collected in step S02 into an autoclave for evaporation at a temperature of 62-68°C for 2-3 hours to obtain a separated resin matrix.

[0018] Furthermore, the thawing process in step S01 is to thaw at 20 to 30° C. for 10 to 15 hours.

[0019] Furthermore, in the step S01, the prepreg is cut into a plurality of 100×200 mm prepreg sheets, and the number of layers of the prepreg is 8 to 12.

[0020] Furthermore, in the step S02, the duration of each static dissolution except the last static dissolution is 10 to 20 minutes, and the duration of the last static dissolution is 10 to 18 hours.

[0021] Furthermore, in step S03, the ultrasonic power of the ultrasonic cleaning instrument is specifically 100-140W, and the ultrasonic frequency is 28KHz-40KHz.

[0022] Furthermore, the prepreg grade is T700 / TRE231.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention discloses a method for preparing a droplet sample by using a microwave curing process, comprising the following steps: taking out a plurality of fiber filaments from a fiber bundle separated from a prepreg and dried, and embedding the fiber filaments into a fiber filament placement groove; setting weights at both ends of the fiber filaments to produce a pre-tightening force for straightening the fiber filaments; taking out an appropriate amount of resin, evenly applying it on the surface of the fiber filaments above the resin holding groove, and standing in an auxiliary carrier for a period of time; and microwave heating the finally obtained droplet sample. The method of the present invention utilizes a method for separating resin and carbon fiber from a carbon fiber prepreg, and proposes a method for preparing a droplet sample for a microwave curing process, which is used to characterize the fiber-resin interface bonding strength of a microwave curing process. The preparation method is simple, the droplet size is controllable, and the evaluation method is closer to the actual working condition. Based on the above, the mechanical behavior and failure mechanism of the fiber and resin interface in the microwave curing process can be explained, which has important economic value and theoretical research significance, and is also the focus and hotspot of research in this field.

[0025] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are used to provide a further understanding of the embodiments of the present invention and constitute a part of the specification. Together with the following specific implementations, they are used to explain the embodiments of the present invention, but do not constitute a limitation on the embodiments of the present invention. In the accompanying drawings:

[0027] Figure 1 is a schematic structural diagram of the auxiliary carrier profile in an embodiment of the present invention;

[0028] Figure 2 It is a schematic diagram of the side structure of a microdroplet sample to be solidified placed in an auxiliary carrier in an embodiment of the present invention. DETAILED DESCRIPTION

[0029] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, but the present invention can be implemented in many different ways as defined and covered by the claims.

[0030] See also Figure 1 and Figure 2 In one embodiment of the present invention, a method for preparing a droplet sample by using a microwave curing process is provided. The droplet sample is a droplet-shaped resin matrix wrapped on a carbon fiber and completely cured (the final shape of the droplet sample is shown in FIG. Figure 1 The method for preparing the droplet sample in the embodiment of the present invention is specifically as follows:

[0031] S1, taking out a plurality of fiber filaments 4 from the carbon fiber bundle separated from the prepreg and dried, and embedding the plurality of fiber filaments 4 one by one into the plurality of fiber filaments placing grooves 1 of the auxiliary carrier 3;

[0032] S2. A weight 5 of 2 to 5 g is set at both ends of each fiber to produce a pre-tightening force to straighten the fiber;

[0033] S3, taking out a proper amount of resin with a needle, and evenly applying it on the surface of the fiber filament above the resin containing tank 2, and controlling the diameter of the droplets to be between 30 and 50 microns, and then leaving the fiber filament 4 after application in the auxiliary carrier 3 for 30 to 50 minutes;

[0034] S4. Open the furnace door, and place the auxiliary carrier 3 embedded with the fiber filaments 4 as a whole into a heating furnace with eight microwave generators. Note that the auxiliary carrier 3 should be padded as a whole or the length of the fiber filaments should be reduced, so that the weight 5 is suspended in the air (to play a pre-tightening role), and relevant microwave shielding measures should be taken. Turn on the microwave heating furnace, and heat the droplet sample in the auxiliary carrier 3 from room temperature to 125-135°C at a heating rate of 1.5-3°C / min, and keep it warm for 120-135 minutes before stopping the heating. Then cool it with the microwave heating furnace, take out the cooled auxiliary carrier 3 from the microwave heating furnace, loosen the weight 5, and take out the droplet sample in the auxiliary carrier.

[0035] In a specific embodiment, the prepreg is a carbon fiber reinforced resin-based composite material with a grade of T700 / TRE231, which is a thermosetting resin-based composite material. In order to obtain carbon fiber filaments, the step of separating fibers from the prepreg is also included before step S1 of this embodiment, specifically:

[0036] S01. Take the prepreg out from the low temperature environment, thaw it at 20-30°C for 10-15h, and cut the thawed prepreg into several 100×200mm prepreg sheets, with 8 to 12 layers of prepreg.

[0037] S02. Tear off the protective sticker on the outer surface of the cut prepreg sheets, and place all the above prepreg sheets in a dissolving container that can hold the prepreg size according to the same fiber direction, pour an appropriate amount of acetone solution into the dissolving container, and let the prepreg sheets stand and dissolve in the acetone solution for a period of time; repeat the dissolution 4 to 6 times so that the resin matrix in the prepreg can be fully dissolved in the acetone solution; wherein, the duration of each standing dissolution except the last standing dissolution is 10 to 20 minutes, and the duration of the last standing dissolution is 10 to 18 hours; the mixed solution of acetone and resin matrix after each dissolution is collected in a beaker for standby use.

[0038] S03. Place the dissolved fiber into an ultrasonic cleaner, and pour an appropriate amount of anhydrous ethanol solution into it, ultrasonically clean the resin matrix and acetone solution remaining on the fiber surface, repeat the cleaning 2 to 3 times, and each cleaning time is 4 to 10 minutes; wherein, the ultrasonic power of the ultrasonic cleaner is specifically 100 to 140 W, and the ultrasonic frequency is 28 KHz to 40 KHz.

[0039] S04, the carbon fibers after ultrasonic cleaning are bundled together with pressure-sensitive tape in the same fiber direction, and placed in an autoclave, the autoclave is heated to 120-150°C at a heating rate of 1-5°C / min, and the temperature is maintained for 2-3 hours, and then naturally cooled to room temperature to obtain dry carbon fibers. Preferably, the autoclave is heated to 130°C at a heating rate of 1°C / min, and is kept at 130°C for 2 hours, the anhydrous ethanol solution attached to the surface of the carbon fibers is evaporated, and the solution is taken out for use, at which point the fibers have been separated.

[0040] S05. Put the beaker containing the mixed solution of acetone and resin matrix collected in step S02 into an autoclave for evaporation at a temperature of 62-68° C. for 2-3 hours to obtain a separated resin matrix. Preferably, the temperature of the autoclave is set to 65° C. and kept warm for 2 hours to completely evaporate the acetone in the mixed solution, and the resin matrix dissolved therein gradually precipitates as the acetone evaporates. The completely separated resin matrix is ​​stored for later use. At this time, the resin matrix has been separated.

[0041] Those skilled in the art will appreciate that the order of step S04 and step S05 in the present invention is not important, and the carbon fiber and resin matrix in step S04 and step S05 only need to be separated before the subsequent preparation of the droplet sample.

[0042] In the embodiment of the present invention, the carbon fiber and the resin matrix separated from the above steps S01 to S05 are used as follows: Figure 1The auxiliary carrier shown is used to prepare the droplet sample. The auxiliary carrier is made of polytetrafluoroethylene material that is wave-transparent but does not reflect microwaves. The auxiliary carrier 3 includes a carrier body, and a plurality of parallel and spaced fiber filament insertion grooves 1 are provided on the surface of the carrier body. A resin receiving groove 2 is provided at the center of each fiber filament insertion groove 1. Both the fiber filament insertion groove 1 and the resin receiving groove 2 are recessed inward from the surface of the carrier body, and the size of the resin receiving groove 2 is set to be slightly larger than the diameter of the droplet. The specific preparation method is: take out a plurality of fiber filaments from a bundle of dried carbon fiber bundles, and embed the plurality of fiber filaments one by one into the plurality of fiber filament insertion grooves 1 of the auxiliary carrier, and set a 3g weight at both ends of each fiber filament to produce a straightening preload force on the fiber filament. Take out an appropriate amount of resin with a needle and apply it to the fiber filament above the resin receiving groove. Let the applied fiber stand in the carrier for 35 minutes. Open the furnace door, then put the whole carrier into the octagonal microwave heating furnace, use a polytetrafluoroethylene block slightly smaller than the auxiliary carrier to pad the bottom of the auxiliary carrier, so that the weight is suspended, close the microwave heating furnace door, seal the reserved hole in the microwave heating furnace with aluminum foil, turn on the microwave heating furnace, and set the following process: heat the droplet sample in the auxiliary carrier from room temperature to 130°C at a heating rate of 2°C / min, stop heating after keeping warm for 120min, and then cool it with the microwave heating furnace, take out the cooled auxiliary carrier from the microwave heating furnace, loosen the weight, and take out the prepared droplet sample. Preferably, the auxiliary carrier can form 4 droplet sample pieces of microwave curing process at one time.

[0043] By preparing droplet samples using the method of the present invention and performing performance tests on the droplet samples, the failure mechanism of the interface between the fiber and the resin can be revealed, and further research can be conducted on how to improve the bonding performance between the fiber and the resin, so as to achieve the purpose of improving the performance of the fiber-reinforced resin-based composite material.

[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a droplet sample using a microwave curing process, characterized in that: The method comprises preparing a droplet sample by using an auxiliary carrier (3), wherein the auxiliary carrier (3) comprises a carrier body, wherein a plurality of fiber thread insertion grooves (1) arranged in parallel and at intervals are arranged on the molding surface of the carrier body, wherein a resin containing groove (2) is arranged at the center of each fiber thread insertion groove (1), and the fiber thread insertion groove (1) and the resin containing groove (2) are both arranged to be recessed inward from the molding surface of the carrier body; the method comprises the following steps: S1, taking out a plurality of fiber filaments (4) from the carbon fiber bundle separated from the prepreg and dried, and embedding the plurality of fiber filaments (4) one by one into a plurality of fiber filament insertion grooves (1) of the auxiliary carrier (3); wherein the grade of the prepreg is T700 / TRE231; S2. A weight (5) of 2 to 5 g is respectively arranged at both ends of each fiber filament (4) to generate a pre-tightening force for straightening the fiber filament (4); S3, taking out a proper amount of resin with a needle, and evenly applying it on the surface of the fiber filaments above the resin holding tank (2), and controlling the diameter of the droplets to be between 30 and 50 microns, and then leaving the fiber filaments (4) after application in the auxiliary carrier (3) for 30 to 50 minutes; S4, placing the auxiliary carrier (3) embedded with the fiber filaments (4) as a whole into a heating furnace with a microwave generator, and leaving the weight (5) suspended in the air, turning on the microwave heating furnace, heating the droplet sample in the auxiliary carrier (3) from room temperature to 130°C at a heating rate of 2°C / min, and stopping heating after keeping the temperature for 120 minutes, and then cooling the auxiliary carrier (3) along with the microwave heating furnace, taking the cooled auxiliary carrier (3) out of the microwave heating furnace, loosening the weight (5), and taking out the droplet sample in the auxiliary carrier; Wherein, the step of separating fibers from the prepreg before step S1 is: S01, taking out the prepreg from the low temperature environment, thawing it at 20-30°C for 10-15h, and cutting the thawed prepreg into a plurality of 100×200mm prepreg sheets, wherein the number of layers of the prepreg is 8-12; S02, tear off the protective stickers on the surfaces of the cut prepreg sheets, and put all the prepreg sheets into a dissolution container in the same fiber direction, pour an appropriate amount of acetone solution into the dissolution container, and let the prepreg sheets stand and dissolve in the acetone solution for a period of time; repeat the dissolution 4 to 6 times, and collect the mixed solution of acetone and resin matrix in a beaker after each dissolution; except for the last standing dissolution, the duration of each standing dissolution is 10 to 20 minutes, and the duration of the last standing dissolution is 10 to 18 hours; S03, placing the dissolved carbon fiber into an ultrasonic cleaner, and pouring an appropriate amount of anhydrous ethanol solution into it, ultrasonically cleaning the acetone and resin matrix mixed solution remaining on the surface of the carbon fiber, repeating the cleaning 2 to 3 times, each cleaning time is 4 to 10 minutes; wherein the ultrasonic power of the ultrasonic cleaner is specifically 100 to 140 W, and the ultrasonic frequency is 28 KHz to 40 KHz; S04, the carbon fibers after ultrasonic cleaning are bundled together with a pressure-sensitive tape in the same fiber direction, and placed in an autoclave, the autoclave is heated to 130° C. at a heating rate of 1° C. / min, and the temperature is maintained at a constant temperature for 2 h, and then naturally cooled to room temperature to obtain a dry carbon fiber bundle; S05, placing the beaker containing the acetone and resin matrix mixed solution collected in step S02 into an autoclave for evaporation at a temperature of 62-68°C for 2-3 hours to obtain a separated resin matrix.