Fully polished glaze slurry, ceramic rock board and preparation method thereof
By using white ore oil-based fully polished glaze slurry and specially made ceramic glaze, combined with digital white glaze ink and polishing processing, the problems of drying and cracking of ceramic rock slabs and mirror polishing are solved, and efficient production of ceramic rock slabs with thickness less than 4mm and Mirror effect.
Patent Information
- Application Number
- CN202310744802.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-06-21
AI Technical Summary
The existing water-based fully-polished glaze slurry will cause dry green bodies to crack in water when decorating ultra-thin ceramic rock slabs, making it difficult to achieve mass production of large-scale mirror polished glazed ceramic rock slabs with a thickness of less than 4mm.
White ore oil is used as the solvent for the fully glaze-polished slurry, combined with quartz, zinc oxide, wollastonite and other materials to prepare the fully glaze-polished glaze and fuse. Through ball milling and roasting treatment, anhydrously fully glaze-polished slurry is formed for decoration. Ceramic rock slabs ensure that their drying process does not crack, and the mirror effect is achieved through digital white glaze ink and independently developed polishing processing equipment.
It effectively solves the problem of drying green-formed ceramic rock slabs caused by water-based fully glaze slurry, and realizes the mirror polishing effect of ceramic rock slabs with a thickness of less than 4mm, which improves the strength and cost-effectiveness of the product.
Smart Images

Figure CN116813200B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ceramic technology, and in particular to a full-polished glaze slurry, a ceramic rock plate and a preparation method thereof. Background Art
[0002] As the latest representative product of ceramic decorative materials, ceramic rock slabs have high density and excellent processing properties such as easy cutting, drilling, and grinding. At the same time, they also have large specifications, diverse colors, high temperature resistance, wear resistance, anti-penetration, acid and alkali resistance, zero formaldehyde, environmental protection and health. They are widely used as home decoration materials, specifically for background walls, cabinets, wardrobes, tea sets, bathroom cabinets, sinks, doors and kitchen stove panels. Among them, ceramic rock slabs used for cabinet and wardrobe decoration generally require the use of thin ceramic rock slabs with a thickness of less than 6mm, especially 3mm thick ultra-thin ceramic rock slab products. Due to its thin thickness, light weight, rich surface patterns, and good physical properties, it is becoming more and more popular. However, the production of ultra-thin ceramic rock slabs with a mirror effect of less than 4mm thickness still has many technical difficulties that need to be overcome. Firstly, if the glazed surface of large-sized glazed ultra-thin ceramic rock slabs with a thickness of less than 4mm is to be mirror-polished, the surface needs to have a thicker transparent glaze layer (thickness > 0.12mm). Using the existing traditional water-based full-polished glaze wet glazing decoration process will cause the dry green body of the large-sized glazed ultra-thin ceramic rock slabs to crack when exposed to water. How to decorate with thicker transparent glaze becomes a difficult problem for the mass production of large-sized mirror-polished glazed ultra-thin ceramic rock slabs with a thickness of less than 4mm. Secondly, since the production difficulty of this type of ceramic rock slab products lies in the fact that the brick body is too thin and has low strength, how to achieve polishing (especially mirror polishing) and how to control the production process from cracking are the key. Therefore, more reasonable design is needed in the body formula as well as the drying, glazing and kiln processes.
[0003] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0004] Based on the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a full-polished glaze slurry, a ceramic rock slab and a preparation method thereof, aiming to solve the problem that the existing use of water-based full-polished glaze slurry will cause the dry green body of the glazed ultra-thin ceramic rock slab to crack when exposed to water.
[0005] The technical solution of the present invention is as follows:
[0006] In a first aspect of the present invention, a full-polished glaze slurry is provided, wherein the slurry comprises the following components in parts by mass:
[0007] 29-35 parts of white mineral oil, 39-50 parts of full-polished glaze, 20-25 parts of frit, and 1-1.5 parts of dispersant.
[0008] Optionally, the full-polished glaze is prepared from raw materials including the following components, measured by mass:
[0009] 3-6 parts of quartz, 2-3.5 parts of zinc oxide, 13-16 parts of wollastonite, 30-33 parts of albite, 10-15 parts of potassium feldspar, 7-9 parts of kaolin, 0.5-2 parts of strontium carbonate, and 6-8 parts of talc.
[0010] Optionally, the chemical composition of the frit includes, by mass:
[0011] SiO2 46-47 parts, Al2O3 26-27 parts, Fe2O3 0-0.1 parts, CaO 17-18 parts, MgO 2.5-3 parts, K2O 2-2.5 parts, Na2O 1-1.5 parts, ZnO 1-2 parts, BaO 0.5-1.0 parts, and reduce by 2.5-3 parts as appropriate.
[0012] Optionally, the dispersant includes at least one of a polyether dispersant, a polyacrylate dispersant, a polyester dispersant, and a polypropylene hydrocarbon dispersant.
[0013] A second aspect of the present invention provides a method for preparing a full-polished glaze slurry, comprising the steps of:
[0014] By weight, 29 to 35 parts of white mineral oil, 39 to 50 parts of full-polished glaze, 20 to 25 parts of frit, and 1 to 1.5 parts of dispersant are mixed and ball-milled to obtain the full-polished glaze slurry.
[0015] Optionally, the method for preparing the full-polished glaze comprises the steps of:
[0016] Mix 3-6 parts of quartz, 2-3.5 parts of zinc oxide, 13-16 parts of wollastonite, 30-33 parts of albite, 10-15 parts of potassium feldspar, 7-9 parts of kaolin, 0.5-2 parts of strontium carbonate and 6-8 parts of talc by weight, and then perform wet ball milling, iron removal and spray granulation in sequence to obtain a powder;
[0017] The powder is calcined at a temperature of 850-950° C. for 2-4 hours and crushed to obtain the full-polished glaze.
[0018] The third aspect of the present invention provides a ceramic rock slab, which includes a green body, a base glaze layer, a pattern decoration layer and a full-polished glaze layer stacked in sequence, wherein the full-polished glaze layer is prepared from the full-polished glaze slurry of the present invention as described above, or the full-polished glaze layer is prepared from the full-polished glaze slurry prepared by the preparation method of the present invention as described above.
[0019] Optionally, the raw materials of the green body include, by weight:
[0020] 10-15 parts of ball clay, 10-25 parts of bentonite, 5-10 parts of kaolin, 15-20 parts of washed mud, 5-10 parts of sericite clay, 30-40 parts of potassium feldspar, 2-4 parts of calcined talc, 7-10 parts of high sodium and high aluminum feldspar powder, 6-10 parts of alumina powder, and 3-5 parts of first composite zirconium powder.
[0021] Optionally, the base glaze layer is prepared from digital white glaze ink, and the digital white glaze ink comprises the following components in parts by mass:
[0022] 57-62 parts of white glaze powder, 55-67 parts of organic solvent, 4.9-8.9 parts of first additive, 0.3-1.0 parts of second additive;
[0023] The white glaze powder comprises the following components:
[0024] The second composite zirconium powder 85-95 parts, bauxite powder 1-3 parts, potassium feldspar 2-5 parts, fused quartz 2-7 parts;
[0025] The second composite zirconium powder includes zirconium oxide powder and zirconium silicate powder, or the second composite zirconium powder includes zirconium oxide powder, zirconium silicate powder and aluminum zirconium composite powder;
[0026] The first auxiliary agent is a dispersant; the second auxiliary agent includes at least one of a leveling agent, a cosolvent, an anti-settling agent, an anti-diffusion agent, and a defoaming agent.
[0027] A fourth aspect of the present invention provides a method for preparing a ceramic rock plate, comprising the steps of:
[0028] providing a blank;
[0029] forming a bottom glaze layer on the green body;
[0030] forming a pattern decoration layer on the base glaze layer;
[0031] Applying full-polishing glaze slurry on the pattern decoration layer, drying, firing, and then polishing to obtain the ceramic rock plate;
[0032] The full-polished glaze slurry is the full-polished glaze slurry described above in the present invention and / or the full-polished glaze slurry prepared by the preparation method described above in the present invention.
[0033] Beneficial effects: The present invention uses white mineral oil as the solvent of the full-polished glaze slurry, that is, the full-polished glaze slurry is a white mineral oil-based full-polished glaze slurry, which does not contain water. When the full-polished glaze slurry is used to decorate ceramic rock panels, especially ultra-thin ceramic rock panels with a thickness of less than 4 mm, the dry green body of the ultra-thin ceramic rock panels will not crack when exposed to water, which effectively solves the problem of the dry green body of the ultra-thin ceramic rock panels decorated with glazes cracking when exposed to water caused by the existing use of water-based full-polished glaze slurry. In addition, the full-polished glaze slurry using white mineral oil as a solvent has a low cost, and during the storage period in the slurry pool, unlike water-based glaze slurry, there is no need to add fungicides or preservatives such as kasone, biguanide, and phenoxyethanol. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the preparation process of the mirror-polished glazed ultra-thin ceramic rock slab in Example 1.
[0035] Figure 2 Figures are particle morphology images of different green powders, where (a) is the particle morphology image of the green powder when the clay raw materials account for 55% of the total raw material mass, (b) is the particle morphology image of the green powder when the clay raw materials account for 35% of the total raw material mass, (c) is the particle morphology image of the green powder when the clay raw materials account for 25% of the total raw material mass, (d), (e), and (f) are enlarged images of the boxed areas in (a), (b), and (c), respectively.
[0036] Figure 3 This is a graph showing the thickness test results of the ceramic rock slab before polishing in Example 1.
[0037] Figure 4 This is the surface SEM image of the green body in Example 1.
[0038] Figure 5 This is a diagram showing the phase analysis results of the ceramic rock slab before polishing in Example 1.
[0039] Figure 6 This is a physical picture of the polished glaze ultra-thin ceramic rock slab with a mirror-like bright effect of 90° glossiness in Example 2.
[0040] Figure 7 This is a real-life picture of the polished glaze ultra-thin ceramic rock slab with a mirror-like soft light effect of 45° glossiness in Example 3. DETAILED DESCRIPTION
[0041] The present invention provides a full-polished glaze slurry, a ceramic rock plate and a preparation method thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0043] The embodiment of the present invention provides a full-polished glaze slurry, which includes the following components in parts by mass:
[0044] 29-35 parts of white mineral oil, 39-50 parts of full-polished glaze, 20-25 parts of frit, and 1-1.5 parts of dispersant.
[0045] In the embodiment of the present invention, white mineral oil is used as the solvent of the full-polished glaze slurry, that is, the full-polished glaze slurry is a white mineral oil-based full-polished glaze slurry, which does not contain water. When the full-polished glaze slurry is used to decorate ceramic rock panels, especially ultra-thin ceramic rock panels with a thickness of less than 4 mm, the dry green body of the ultra-thin ceramic rock panels will not crack when exposed to water, which effectively solves the problem of the dry green body of the ultra-thin glazed ceramic rock panels cracking when exposed to water caused by the existing use of water-based full-polished glaze slurry. In addition, the full-polished glaze slurry with white mineral oil as the solvent has a low cost, and during the storage period in the slurry pool, unlike water-based glaze slurry, there is no need to add fungicides or preservatives such as kasone, biguanide, and phenoxyethanol.
[0046] In the present embodiment, the white mineral oil is a colorless, tasteless, odorless, non-corrosive, translucent viscous special mineral oil that has been ultra-deeply refined (deep hydrofining removes impurities such as aromatic hydrocarbons, sulfur, nitrogen and oxygen), and does not contain any additive moisture and mechanical impurities. The composition of white mineral oil is basically saturated hydrocarbons (cycloalkanes and alkanes), and its impurity content such as aromatic hydrocarbons, nitrogen, oxygen, and sulfur is very low (approximately zero), insoluble in water and ethanol, soluble in volatile oils, and miscible in most non-volatile oils (excluding castor oil). The relative molecular mass of white mineral oil is 300-400, which belongs to the lubricating oil fraction. Liquid white mineral oil has the following advantages: ① It has good chemical inertness, stability and excellent oxidation, heat, light and other stability; ② It has a certain antibacterial effect, and its corresponding full-polished glaze slurry is not easily contaminated by pathogens and molds and deteriorated; ③ Compared with other organic solvents, the viscosity of white mineral oil is 3-15mPa·s, which meets the needs of ceramic rock slab glaze decoration and has a high cost performance. It has obvious cost advantages, which is only about one-third of the price of other organic solvents, and is more in line with the requirements of mass industrial use.
[0047] In this embodiment, the white mineral oil can be industrial-grade white mineral oil of Total of France, also commonly known as white oil; its model is divided according to different viscosity properties, and is roughly divided into 3#, 5#, 7#, 10#, 15#, 26#, 32#, 48#, 68#, 90#, 100#, etc. According to the different glazing decoration processes (spray glaze and pour glaze), the preferred model of white mineral oil is also different; for the spray glaze decoration process, 7# white mineral oil is preferred; for the pour glaze decoration process, 10# white mineral oil is preferred. In the following embodiments of the present invention, 10# white mineral oil is selected for the pour glaze decoration process.
[0048] In some embodiments, the full-polished glaze is prepared from raw materials including the following components, in parts by mass:
[0049] 3-6 parts of quartz, 2-3.5 parts of zinc oxide, 13-16 parts of wollastonite, 30-33 parts of albite, 10-15 parts of potassium feldspar, 7-9 parts of kaolin, 0.5-2 parts of strontium carbonate, and 6-8 parts of talc.
[0050] In this embodiment, the full-polished glaze mainly uses raw materials with low burning loss, and uses composite flux (zinc, calcium, sodium, potassium, strontium, etc.) to ensure that the glaze can achieve the best transparency and transparency within a wider firing range.
[0051] In some embodiments, the chemical composition of the frit includes, by weight:
[0052] SiO2 46-47 parts, Al2O3 26-27 parts, Fe2O3 0-0.1 parts, CaO 17-18 parts, MgO2.5-3 parts, K2O 2-2.5 parts, Na2O 1-1.5 parts, ZnO 1-2 parts, BaO 0.5-1.0 parts, and 2.5-3 parts less. The frit is a high-temperature frit powder, specifically a high-aluminum-calcium transparent frit, which can achieve sintering and melting performance synchronously with the full-polished glaze during the firing process of the ceramic rock plate, and will not cause defects such as pinholes and insufficient transparency due to premature melting or incomplete melting.
[0053] In some embodiments, the dispersant includes at least one of a polyether dispersant, a polyacrylate dispersant, a polyester dispersant, and a polypropylene hydrocarbon dispersant. These dispersants are super wetting dispersants with good dispersibility. Among them, the polyether dispersant is a high molecular polymer containing a polyamine anchoring group (such as Xinchi 926 super dispersant, YY502 produced by Guangzhou Yuantai Synthetic Materials Co., Ltd., etc.), with a purity of 99.5%, a flash point greater than 150°C, and has the following characteristics: ① It has an ultra-long molecular chain structure, which can quickly and fully wet the particles and greatly improve the surface properties of the particles; ② The polyamine anchoring group has a strong affinity with the particles, which can greatly increase the solid particle content in the full-polished glaze slurry, thereby saving the glaze slurry processing and energy consumption costs; ③ It has a very strong dispersing ability to prevent the particles from secondary agglomeration and flocculation, ensuring uniform and stable dispersion; ④ It can greatly reduce the viscosity of the full-polished glaze slurry and improve its flow properties, so that it can meet the glazing decoration performance requirements.
[0054] The embodiment of the present invention also provides a method for preparing a full-polished glaze slurry, which comprises the steps of:
[0055] By weight, 29 to 35 parts of white mineral oil, 39 to 50 parts of full-polished glaze, 20 to 25 parts of frit, and 1 to 1.5 parts of dispersant are mixed and ball-milled to obtain the full-polished glaze slurry.
[0056] In this embodiment, the mixture is mixed according to the full-polished glaze slurry formula ratio. For example, the white mineral oil required by the formula can be first added to a 1.5T intermittent ball mill cylinder, and then the full-polished glaze and frit are gradually added, and finally the dispersant is added for ball milling. The specific chemical composition of the frit is described above.
[0057] In some embodiments, the full-polished glaze slurry has a specific gravity of 1.70 to 1.80, a flow rate of 20 to 45 seconds, a viscosity of 75 to 100 mPa·s, and a fineness of passing through a 325-mesh sieve (the residue on the sieve is 0).
[0058] In some embodiments, the method for preparing the full-polished glaze comprises the steps of:
[0059] Mix 3-6 parts of quartz, 2-3.5 parts of zinc oxide, 13-16 parts of wollastonite, 30-33 parts of albite, 10-15 parts of potassium feldspar, 7-9 parts of kaolin, 0.5-2 parts of strontium carbonate and 6-8 parts of talc by weight, and then perform wet ball milling, iron removal and spray granulation in sequence to obtain a powder;
[0060] The powder is calcined at a temperature of 850-950° C. for 2-4 hours and crushed to obtain the full-polished glaze.
[0061] In this embodiment, the effects of roasting are: ① After roasting, it can be ensured that the raw materials do not contain moisture, and at the same time, the hydroxyl groups in the raw materials are removed, so that the white mineral oil and the full-polished glaze can be quickly mixed and evenly integrated during grinding and mixing, and it is not easy to produce stratification, which solves the problem that conventional water-based glaze slurry needs to add sodium carboxymethyl cellulose, kaolin, ball clay and other materials to improve the suspension performance of the glaze slurry; ② After roasting, the raw materials are easy to grind and crush, which shortens the grinding time of the glaze slurry, the processing efficiency can be increased by more than 30%, and the glaze slurry performance is better.
[0062] Preferably, the particle size D97 of these raw materials for preparing the full-polished glaze is ≤100 μm, which can shorten the ball milling time, help improve the processing efficiency of the full-polished glaze slurry, and reduce the impact of the ball milling temperature on the slurry performance.
[0063] The embodiment of the present invention also provides a ceramic rock board, which includes a green body, a base glaze layer, a pattern decoration layer and a full-polished glaze layer stacked in sequence, wherein the full-polished glaze layer is prepared from the full-polished glaze slurry described in the embodiment of the present invention, or the full-polished glaze layer is prepared from the full-polished glaze slurry prepared by the preparation method described in the embodiment of the present invention, and the thickness of the ceramic rock board is less than 4 mm. The ultra-thin ceramic rock board provided in this embodiment will not crack, has high strength, and has a rupture modulus of 57 to 65 MPa (the rupture modulus of existing ceramic rock boards is 45 to 50 MPa).
[0064] In some embodiments, the raw materials of the green body include, by weight:
[0065] 10-15 parts of ball clay, 10-25 parts of bentonite, 5-10 parts of kaolin, 15-20 parts of washed mud, 5-10 parts of sericite clay, 30-40 parts of potassium feldspar, 2-4 parts of calcined talc, 7-10 parts of high sodium and high aluminum feldspar powder, 6-10 parts of alumina powder, and 3-5 parts of first composite zirconium powder.
[0066] In this embodiment, a large amount of bentonite is used in the raw materials of the green body, which ensures the drying temperature of the ultra-thin ceramic rock plate, is conducive to the decoration of patterns and glazes, and can achieve fast firing without black heart defects in the green body. The green body provided in this embodiment has high strength.
[0067] The ball clay may be specifically strong plastic ball clay, which is a highly plastic clay rich in organic matter, a secondary clay, with a plasticity index Ip>16, and is mainly composed of kaolin components, associated with quartz and mica minerals, and a carbon content of ≤0.5%; the introduction of strong plastic ball clay is conducive to ensuring that there are no cracking defects after the green body is dried and glazed, and after firing, the amount of mullite crystal phase in the ceramic rock plate green body can be increased and the green body can be ensured to have no black heart phenomenon. Specifically, the strong plastic ball clay includes the following chemical components by mass:
[0068] SiO2 49-55 parts, Al2O3 30-34 parts, Fe2O3 0-0.5 parts, CaO 0-0.1 parts, MgO 0-0.2 parts, K2O 0.5-1.3 parts, Na2O 0.2-0.4 parts, TiO2 0-0.3 parts, C 0-1.0 parts, and 10-13 parts less as appropriate.
[0069] Bentonite is a clay rock, also known as montmorillonite clay rock. It is easily exchanged by other cations and can be modified. It has good ion exchange, strong hygroscopicity and swelling properties. It can be dispersed into gel and suspension in water medium and is called "universal soil". Bentonite can be divided into sodium bentonite (alkaline soil), calcium bentonite (alkaline earth soil, including calcium sodium and calcium magnesium, etc.), natural bleaching earth (acidic soil or acidic white clay), lithium bentonite, etc.; in the embodiment of the present invention, sodium bentonite and lithium bentonite are preferably used, and the bentonite is composed of 50 to 75 parts by mass of sodium bentonite and 25 to 50 parts by mass of lithium bentonite. Among them,
[0070] The sodium bentonite comprises the following chemical components by weight:
[0071] SiO2 65-69 parts, Al2O3 14-15.6 parts, Fe2O3 0-0.5 parts, TiO2 0-0.06 parts, CaO 3.5-4.5 parts, MgO 2-4 parts, K2O 0.1-0.2 parts, Na2O 0.1-0.4 parts, loss on ignition 10-13 parts.
[0072] The specific surface area of lithium-based bentonite is 80-100m 2 / g, made of natural bentonite modified by lithium carbonate, including the following chemical components by mass: SiO2 65-69 parts, Al2O3 14-15.6 parts, Fe2O3 0-0.5 parts, TiO2 0-0.06 parts, CaO 3.5-4.5 parts, MgO 2-4 parts, K2O 0.1-0.2 parts, Li2O0.1-0.4 parts, and ignition loss 10-13 parts.
[0073] The carbon content in kaolin is ≤0.2%. The introduction of kaolin can ensure good sintering performance of the green body, fast sintering and no black heart phenomenon.
[0074] Washed mud refers to the mud obtained by washing some relatively poor quality clay raw materials with water, removing impurities (such as branches, roots, large solid objects, etc.), and filtering them layer by layer with filter cloth of pressing equipment. Its whiteness is 84.7°. By mass, the main chemical components of the washed mud include: SiO2 46-48.07 parts, Al2O3 36-38 parts, K2O 0.35-0.38 parts, Na2O 0.20-0.22 parts, Fe2O3 0-0.3 parts, TiO2 0-0.07 parts, CaO 0-0.11 parts, MgO 0-0.08 parts, and 5-6.5 parts less. Washed mud is beneficial to increase the amount of mullite crystal phase in the green body after firing, and enhance the strength and toughness of ceramic rock plate.
[0075] Sericite clay is white and fine-grained, and has some characteristics of clay minerals (such as viscosity). It has good dispersion and suspension properties in aqueous slurry liquids. Its main components include: SiO2 51-53 parts, Al2O3 29.5-33.65 parts, K2O 7.5-8.5 parts, Na2O 3.2-4.0 parts, Fe2O3 0-0.2 parts, and 5-6.5 parts as appropriate. Sericite clay is beneficial to improving the suspension properties of the green body slurry and the aluminum content in the green body. After firing, it can increase the number of mullite crystal phases in the green body and enhance the strength and toughness of the ceramic rock plate.
[0076] Potassium feldspar can be specifically high white potassium feldspar, whose Mohs hardness is greater than level 6 and whose fineness is 30-80 meshes; the introduction of high white potassium feldspar is conducive to increasing the sintering temperature of the green body and ensuring that the green body has a high whiteness. Specifically, by weight, the chemical composition of the high white potassium feldspar includes:
[0077] SiO2 56-59 parts, Al2O3 27-30 parts, Fe2O3 0-0.7 parts, CaO 0-0.07 parts, MgO 0-0.3 parts, K2O 4-5 parts, Na2O 0.3-0.5 parts, TiO2 0-0.1 parts, C 0-0.1 parts, and reduce by 3-5 parts as appropriate.
[0078] The high sodium and high aluminum feldspar powder comprises the following chemical components by mass:
[0079] SiO2 67-70 parts, Al2O3 18-20 parts, Fe2O3 0-0.1 parts, K2O 0.1-0.4 parts, Na2O 9.5-11.5 parts, TiO2 0-0.05 parts, CaO 0-0.11 parts, MgO 0.2-0.4 parts, and 0.4-0.7 parts can be reduced as appropriate.
[0080] The alumina powder can specifically be α-alumina powder, and its particle size is 1.0 to 2.0 microns; the α-alumina powder acts as a skeleton, which can effectively improve the strength of the finished ceramic rock slab, thereby facilitating the paving performance of the ceramic rock slab at the terminal market.
[0081] The first composite zirconium powder comprises 50-70 parts of zirconium oxide powder, 10-20 parts of zirconium silicate powder, and 20-30 parts of aluminum-zirconium composite powder, wherein the chemical composition of the aluminum-zirconium composite powder comprises:
[0082] SiO2 21.16~23.23 parts, Al2O3 43.04~45.35 parts, Fe2O3 0.37~0.46 parts, CaO 0.35~0.38 parts, MgO 0.1~0.4 parts, K2O 0.2~0.3 parts, Na2O 1.5~2.0 parts, TiO2 0.15~0.3 parts, ZrO2 28~29 parts, and reduce 1.5~1.8 parts as appropriate.
[0083] In some embodiments, the base glaze layer is prepared from digital white glaze ink, and the digital white glaze ink includes the following components in parts by mass:
[0084] 57-62 parts of white glaze powder, 55-67 parts of organic solvent, 4.9-8.9 parts of first additive, 0.3-1.0 parts of second additive;
[0085] The white glaze powder comprises the following components:
[0086] The second composite zirconium powder 85-95 parts, bauxite powder 1-3 parts, potassium feldspar 2-5 parts, fused quartz 2-7 parts;
[0087] The second composite zirconium powder includes zirconium oxide powder and zirconium silicate powder, or the second composite zirconium powder includes zirconium oxide powder, zirconium silicate powder and aluminum zirconium composite powder;
[0088] The first auxiliary agent is a dispersant; the second auxiliary agent includes at least one of a leveling agent, a cosolvent, an anti-settling agent, an anti-diffusion agent, and a defoaming agent.
[0089] In this embodiment, the three raw materials of bauxite powder, potassium feldspar and fused quartz can form a SiO2-Al2O3-K2O system, ensuring that the white glaze is in a better sintering state after firing, which is beneficial to the coloring of various ceramic color inks on its surface. Therefore, in this embodiment, decorating the green body layer with digital white ink (with high white function) can improve the covering power of the green body color and enhance the coloring ability of the pattern decoration layer ink; at the same time, in this embodiment, the white glaze powder has an expansion system matching the green body, and the expansion coefficient characteristics of the digital white ink are used as a transition between the green body and the full-polished glaze to achieve the uniformity of the brick shape.
[0090] In some embodiments, the second composite zirconium powder includes 50-70 parts of zirconium oxide powder, 10-20 parts of zirconium silicate powder, and 20-30 parts of aluminum-zirconium composite powder by weight. This ratio can ensure that the white glaze has a more suitable expansion coefficient.
[0091] In some embodiments, the chemical composition of the aluminum-zirconium composite powder includes, by mass:
[0092] SiO2 21.16~23.23 parts, Al2O3 43.04~45.35 parts, Fe2O3 0.37~0.46 parts, CaO 0.35~0.38 parts, MgO 0.1~0.4 parts, K2O 0.2~0.3 parts, Na2O 1.5~2.0 parts, TiO2 0.15~0.3 parts, ZrO2 28~29 parts, and reduce 1.5~1.8 parts as appropriate.
[0093] In some embodiments, the bauxite ore powder is diaspore-type bauxite ore powder, and the diaspore-type bauxite ore powder loses water upon heating to generate anhydrous α-Al2O3 and corundum.
[0094] In some embodiments, the organic solvent includes an ester solvent, and the ester solvent includes at least one of diethyl hexyl adipate, isooctyl palmitate, isopropyl laurate, isooctyl laurate, myristic acid ester, triethylene glycol diethyl hexyl ester, and D120 solvent oil, but is not limited thereto.
[0095] In some embodiments, the dispersant includes at least one of Huihong HP166, Huihong HP1068, Lubrizol Solsperse 13940, BYKJET-9142, polyvinyl acetate, polyvinyl versatate, and isopropyl alcohol, but is not limited thereto. These dispersants are hyperdispersants with good dispersing effects.
[0096] In some embodiments, the leveling agent includes polyether-modified siloxane, and specifically may include at least one of BYK306, BYK333, and Levaslip 8629, but is not limited thereto.
[0097] In some embodiments, the co-solvent includes urea or ethylene urea, but is not limited thereto.
[0098] In some embodiments, the anti-settling agent includes at least one of polyamide wax and oxidized polyethylene. Specifically, the anti-settling agent includes at least one of Disparlon NS-5501 and Disparlon 6650, but is not limited thereto.
[0099] In some embodiments, the anti-diffusion agent includes at least one of polypropylene glycol 2000, isomeric decanol polyoxyethylene ether E-05, and glycerol polyoxypropylene ether HSH-330, but is not limited thereto.
[0100] In some embodiments, the defoaming agent is a polymer defoaming agent that does not contain silicone, and specifically may include at least one of BYK051, BYK052, BYK065, BYK066N, and BYK088, but is not limited thereto.
[0101] The present invention also provides a method for preparing the ceramic rock plate as described above in the present invention, which comprises the steps of:
[0102] S1. providing a blank;
[0103] S2, forming a bottom glaze layer on the green body;
[0104] S3, forming a pattern decoration layer on the base glaze layer;
[0105] S4. Apply full-polished glaze slurry on the pattern decoration layer, dry and fire it, and then polish it to obtain the ceramic rock plate; the full-polished glaze slurry is the full-polished glaze slurry described above in the embodiment of the present invention and / or the full-polished glaze slurry prepared by the preparation method described above in the embodiment of the present invention.
[0106] In step S1, in some embodiments, the method for preparing the green body comprises the steps of:
[0107] S11. The raw materials of the blank of the present invention in the above-mentioned mass parts are sent into a ball mill for wet ball milling to obtain blank slurry, the mass content of water in the blank slurry is 35-37%, the specific gravity of the blank slurry is 1.75-1.78, the ball discharge flow rate of the blank slurry is 75-100s, the fineness of the blank slurry is 1.5-2.0% of the mass of the blank slurry remaining on the 325 mesh sieve, and the particle size D50 of the solid particles in the blank slurry is 7.5-8.5μm.
[0108] S12, aging and homogenizing the blank slurry, and spray granulating to obtain the blank powder; the particle gradation (standard sieve) of the blank powder is: 20 mesh sieve residue ≤ 0.5wt%, 40 mesh sieve residue 70-75wt%, 60 mesh sieve residue 15-20wt%, 80 mesh sieve residue 3-5wt%, 100 mesh sieve residue ≤ 1wt%, 120 mesh sieve residue ≤ 0.5wt%, the bulk density of the blank powder is 0.95-0.98g / mL (bulk density is the weight of the blank powder per unit volume), and the moisture content of the blank powder is 6.6-7.3%; the particles of the blank powder are solid spheres with a relatively smooth surface;
[0109] S13, aging the green body powder for more than 48 hours (so that the moisture content of the green body powder is 6.1-6.5%), and then pressing and forming (specifically, the aged green body powder can be transported to the hopper on the top of the press, and pressed by a SYSTEM frameless belt press at a pressure of 360-420 bar) to obtain a green body (volume density of 1.900-1.914 g / cm 3 );
[0110] S14, drying the green body to obtain a green body (specifically, the green body can be transported to a 3-5 layer roller kiln for drying, the drying temperature is 140-160°C, the drying time is 100-120 min, and the green body with a strength of 4.5-5.5 MPa and a moisture content of less than 0.3% is obtained; the green body specifications are: length of more than 2.8 m, width of 1.0 m, thickness <4 mm).
[0111] Furthermore, after completing the above steps S11-S14, a step of brushing and polishing the surface of the blank can be performed according to actual needs. Specifically, the blank is subjected to physical surface brushing treatment by using a blank polishing machine, the purpose of which is to remove impurities on the surface of the blank.
[0112] In step S2, the step of forming a base glaze layer on the green body specifically includes:
[0113] Mixing the raw materials in the digital white glaze ink in parts by weight to obtain digital white glaze ink;
[0114] The digital white glaze ink is applied to the green body to form a base glaze layer.
[0115] Specifically, a digital inkjet printer (the nozzle model is Xaar GS40, Starlight 1024HF) can be used to apply the digital white glaze ink to the blank.
[0116] In step S3, the step of forming a pattern decoration layer on the base glaze layer specifically includes:
[0117] An inkjet printer is used to print patterns on the base glaze layer to form a pattern decoration layer.
[0118] Among them, the order of ink colors installed on the inkjet machine is: cyan → purple blue → red brown → dark brown → wrapped red → orange → lemon yellow → green → blue black → red black, and the inkjet printing nozzle model is Xaar GS12 or Starlight 1024M.
[0119] In step S4, in some embodiments, the step of applying full-polishing glaze slurry on the pattern decoration layer, drying, firing, and then polishing to obtain the ceramic rock plate specifically includes:
[0120] The above-mentioned full-polished glaze slurry is mixed with 400-500g / m2 The glaze amount is applied to the pattern decoration layer, dried at a temperature of 105 to 205° C. for 5 to 8 minutes, and then fired at a temperature of 1185 to 1190° C. for 85 to 95 minutes;
[0121] Then polishing is performed to obtain a ceramic rock plate with a mirror effect (volume density of 2.56-2.60 g / cm 3 , water absorption rate is 0.019~0.023%, modulus of rupture is 57~65MPa, specification size is above 1000mm×2800mm, thickness is less than 4mm).
[0122] Polishing can be performed using a self-developed ceramic rock plate surface polishing processing device (see Chinese invention patent CN215547718U) to stably achieve two mirror effects on the glaze surface of the ultra-thin ceramic rock plate: soft light (glossiness of 38-52°) and bright light (glossiness of 90-95°). Different polishing moduli and polishing parameters are selected according to the different glossiness effects required, as shown in Table 1 below. Among them, elastic modules with different mesh sizes are made of diamond abrasives with different fineness and polymer resin, and fiber flat modules with different mesh sizes are made of diamond abrasives with different fineness and polymer brushed fibers.
[0123] Table 1 Polishing parameters corresponding to different glossiness effects achieved by mirror polishing
[0124]
[0125]
[0126] Of course, the present invention is not limited to specific polishing equipment and methods. Any equipment and method that can polish thin rock slabs with a thickness of less than 4 mm is applicable to the present invention.
[0127] The present invention will be further described below by means of specific examples.
[0128] In the following examples, the chemical composition of the frit used, measured by mass, includes:
[0129] SiO2 46.5 parts, Al2O3 26.5 parts, Fe2O3 0.06 parts, CaO 17.5 parts, MgO 2.8 parts, K2O 2.3 parts, Na2O 1.2 parts, ZnO 1.5 parts, BaO 0.8 parts, and 2.8 parts less as appropriate.
[0130] In the following examples, the white mineral oil used is industrial grade white mineral oil of Total Company of France, model 10#.
[0131] In the following examples, the chemical components of the strong plastic ball clay used include, by weight:
[0132] SiO2 52 parts, Al2O3 32 parts, Fe2O3 0.2 parts, CaO 0.1 parts, MgO 0.1 parts, K2O 0.9 parts, Na2O 0.3 parts, TiO2 0.2 parts, C 1.0 parts, and 10 parts less as appropriate.
[0133] The bentonite used in the following implementation includes 60 parts by mass of sodium bentonite and 40 parts by mass of lithium bentonite, wherein, by mass, the sodium bentonite includes the following chemical components:
[0134] SiO2 67 parts, Al2O3 15 parts, Fe2O3 0.3 parts, TiO2 0.03 parts, CaO 4 parts, MgO 3 parts, K2O 0.2 parts, Na2O 0.3 parts, ignition loss 10 parts.
[0135] Calculated by mass, the lithium-based bentonite includes the following chemical components: 67 parts of SiO2, 15 parts of Al2O3, 0.3 parts of Fe2O3, 0.03 parts of TiO2, 4 parts of CaO, 3 parts of MgO, 0.2 parts of K2O, 0.3 parts of Li2O, and 10 to 13 parts of loss on ignition.
[0136] In the following embodiments, the water-washed mud used includes the following chemical components, calculated by mass: 47 parts of SiO2, 37 parts of Al2O3, 0.36 parts of K2O, 0.21 parts of Na2O, 0.15 parts of Fe2O3, 0.04 parts of TiO2, 0.06 parts of CaO, 0.04 parts of MgO, and 6 parts less.
[0137] In the following embodiments, the sericite clay material used includes the following chemical components, calculated by mass: 52 parts of SiO2, 32 parts of Al2O3, 8 parts of K2O, 3.5 parts of Na2O, 0.1 parts of Fe2O3, and 5 parts of Fe2O3.
[0138] In the following examples, the high-white potassium feldspar used includes the following chemical components by weight:
[0139] SiO2 56 parts, Al2O3 30 parts, Fe2O3 0.4 parts, CaO 0.03 parts, MgO 0.2 parts, K2O 5 parts, Na2O 0.3 parts, TiO2 0.1 parts, C 0.05 parts, and reduce by 3 parts as appropriate.
[0140] In the following examples, the high sodium and high aluminum feldspar powder used includes the following chemical components by weight:
[0141] SiO2 68 parts, Al2O3 19 parts, Fe2O3 0.1 parts, K2O 0.2 parts, Na2O 10 parts, TiO2 0.03 parts, CaO 0.06 parts, MgO 0.3 parts, and 0.4 parts less as appropriate.
[0142] In the following examples, the white glaze powder includes the following components by weight:
[0143] 90 parts of composite zirconium powder, 2 parts of bauxite powder, 3 parts of potassium feldspar, and 5 parts of fused quartz.
[0144] In the following examples, the composite zirconium powder used includes 60 parts of zirconium oxide powder, 15 parts of zirconium silicate powder, and 25 parts of aluminum zirconium composite powder, calculated by mass. The chemical composition of the aluminum zirconium composite powder includes:
[0145] SiO2 22 parts, Al2O3 44 parts, Fe2O3 0.42 parts, CaO 0.37 parts, MgO 0.1 parts, K2O 0.3 parts, Na2O 2.0 parts, TiO2 0.3 parts, ZrO2 29 parts, and reduce by 1.5 parts as appropriate.
[0146] Example 1
[0147] (1) A method for preparing a full-polished glaze, comprising the steps of:
[0148] By weight, 6 parts of quartz, 2 parts of zinc oxide, 16 parts of wollastonite, 33 parts of albite, 10 parts of potassium feldspar, 9 parts of kaolin, 2 parts of strontium carbonate, and 8 parts of talc were mixed, and then wet-milled to obtain a slurry (fineness is to pass through a 325-mesh sieve);
[0149] Then the slurry is filtered through a 120-mesh sieve to remove iron, and then spray granulated to obtain a powder;
[0150] The powder is put into a sagger, fired at 850° C. for 3 hours, and crushed to obtain the full-polished glaze.
[0151] (2) A method for preparing a full-polished glaze slurry, comprising the steps of:
[0152] By mass, add 29 parts of white mineral oil to a 1.5T intermittent ball mill cylinder, then gradually add 50 parts of full-polish glaze and 20 parts of frit, and finally add 1.5 parts of YY502 super dispersant for ball milling to obtain full-polish glaze slurry;
[0153] The specific gravity of the full-polished glaze slurry is 1.8, the flow rate is 21s, the viscosity is 98mPa·s, and the fineness is such that it can pass through a 325-mesh sieve (the residue on the sieve is 0).
[0154] (3) A method for preparing a mirror-polished glazed ultra-thin ceramic rock plate, such as Figure 1 As shown, the steps include:
[0155] a. Preparation of green body:
[0156] By weight, 10 parts of superplastic ball clay, 25 parts of bentonite, 5 parts of raw kaolin, 20 parts of washed mud, 5 parts of sericite clay, 30 parts of high white potassium feldspar, 2 parts of calcined talc, 10 parts of high sodium high aluminum feldspar powder, 6 parts of α-alumina powder, and 5 parts of composite zirconium powder are mixed, and sent into a three-stage continuous ball mill for wet ball milling (coarse grinding and fine grinding) to obtain a blank slurry, wherein the mass content of water in the blank slurry is 36%, the specific gravity of the blank slurry is 1.75, the ball outlet flow rate is 90s, the fineness is 1.5% of the mass of the blank slurry remaining on the 325 mesh sieve, and the particle size D50 of the solid particles in the blank slurry is 8μm;
[0157] The blank slurry is stored in an underground slurry pool for aging and homogenization for 24 hours, and then sent to a drying tower equipped with 24 spray guns by a blocking pump for powder spraying and granulation, and the blank powder is obtained at the bottom of the spray tower; the particle gradation (standard sieve) of the blank powder is: 20 mesh upper sieve residue ≤0.5wt%, 40 mesh upper sieve residue 70-75wt%, 60 mesh upper sieve residue 15-20wt%, 80 mesh upper sieve residue 3-5wt%, 100 mesh upper sieve residue ≤1wt%, 120 mesh upper sieve residue ≤0.5wt%, the bulk density of the blank powder is 0.96g / mL, and the moisture content of the blank powder is 6.6%; the particles of the blank powder are solid spherical with a relatively smooth surface, such as Figure 2 As shown in (a) and (d); in the green body of this embodiment, the clay raw materials account for 55% of the total raw material mass, and under the same mud properties and powder making process conditions, when the proportion of clay raw materials decreases, the sphericity, particle size distribution uniformity, and surface finish of the prepared powder become worse, the larger the angle of repose, and the lower the fluidity index. Therefore, the higher the proportion of clay raw materials, the better the sphericity, particle size distribution uniformity, and surface finish of the prepared powder, the smaller the angle of repose, and the higher the fluidity index. When the clay raw materials account for 35% and 25% of the total raw material mass, the particle morphology of the green body powder is as follows: Figure 2 When the clay raw materials in the green body account for 55%, 35%, and 25% of the total raw materials, the properties of the green body powder are shown in Table 2 below.
[0158] Table 2 Performance data of green powder
[0159]
[0160]
[0161] The green body powder was conveyed to the powder bin by belt for aging for 48 hours (so that the moisture content of the green body powder was 6.1%), and then conveyed to the top hopper of the press, and pressed by SYSTEM frameless belt press at a pressure of 360 bar to obtain a green body (volume density of 1.9 g / cm 3 );
[0162] The green body was transported to a roller kiln for drying at a drying temperature of 150°C for 110 minutes, and a body with a strength of 5 MPa and a moisture content of less than 0.3% was obtained. The specifications of the obtained body were: length 2.8 m, width 1.0 m, and thickness <4 mm.
[0163] The surface of the green body is physically polished and brushed by a polishing machine to remove impurities on the surface of the dry green body.
[0164] b. Digital white glaze ink decoration
[0165] 57 parts of white glaze powder, 67 parts of isooctyl laurate, 4.9 parts of Huihong HP166, 0.25 parts of BYK306, 0.15 parts of polyamide wax, 0.3 parts of polypropylene glycol 2000, and 0.1 parts of BYK051 were mixed to obtain digital white glaze ink;
[0166] The digital white glaze ink is decorated on the blank by using a digital inkjet machine (the nozzle model is Xaar GS40), and after drying, a base glaze layer is formed.
[0167] c. Pattern decoration
[0168] The pattern is inkjet printed on the base glaze layer. The order of ink colors installed on the inkjet machine is: cyan → purple blue → red brown → dark brown → wrapped red → orange → lemon yellow → green → blue black → red black. The inkjet printing nozzle model is Xaar GS12. After drying, a pattern decoration layer is formed.
[0169] d. Full glaze decoration
[0170] 400g / m 2 The glaze amount is 100%, and the full-polished glaze slurry is applied to the pattern decoration layer in a pouring glaze manner; the semi-finished product is transported to a glaze line dryer for drying, the drying time is 8 minutes, and the drying temperature is 150°C;
[0171] Then it is sent to the firing kiln (the length of the kiln is 300m, the internal width of the kiln is 2.2m) for firing, fired at 1185℃ for 90min, and a ceramic rock plate is obtained, the size of which is 1000mm×2800mm, and the thickness is less than 4mm (such as Figure 3 As shown), the volume density is 2.56g / cm 3The water absorption rate is 0.019%, and the microstructure of the green body pores (SEM image) is as follows Figure 4 The results of phase analysis (semi-quantitative) are shown in Figure 5 And as shown in Table 3.
[0172] Table 3 Phase analysis results
[0173]
[0174] e. Polishing
[0175] The ceramic rock slab surface polishing processing device independently developed by the company (see Chinese invention patent CN215547718U) is used for polishing to obtain a polished glazed ultra-thin ceramic rock slab with a mirror-like bright effect of 95° glossiness and a rupture modulus of 65MPa.
[0176] Example 2
[0177] (1) A method for preparing a full-polished glaze, comprising the steps of:
[0178] By weight, 3 parts of quartz, 3.5 parts of zinc oxide, 13 parts of wollastonite, 30 parts of albite, 15 parts of potassium feldspar, 7 parts of kaolin, 0.5 parts of strontium carbonate, and 6 parts of talc were mixed, and then wet-milled to obtain a slurry (fineness is to pass through a 325-mesh sieve);
[0179] Then the slurry is filtered through a 120-mesh sieve to remove iron, and then spray granulated to obtain a powder;
[0180] The powder is put into a sagger, fired at 900° C. for 3 hours, and crushed to obtain a fully polished glaze.
[0181] (2) A method for preparing a full-polished glaze slurry, comprising the steps of:
[0182] By mass, 35 parts of white mineral oil were added to a 1.5T intermittent ball mill cylinder, and then 39 parts of full-polished glaze and 25 parts of frit were gradually added, and finally 1 part of YY502 super dispersant was added for ball milling to obtain a full-polished glaze slurry. The full-polished glaze slurry has a specific gravity of 1.7, a flow rate of 45s, a viscosity of 80mPa·s, and a fineness of passing through a 325 mesh sieve (the residue on the sieve is 0).
[0183] (3) A method for preparing a mirror-polished glazed ultra-thin ceramic rock plate, comprising the steps of:
[0184] a. Preparation of green body:
[0185] By weight, 15 parts of super-plastic ball clay, 10 parts of bentonite, 10 parts of raw kaolin, 15 parts of washed mud, 10 parts of sericite clay, 40 parts of high white potassium feldspar, 4 parts of calcined talc, 7 parts of high sodium high aluminum feldspar powder, 10 parts of α-alumina powder, and 3 parts of composite zirconium powder are mixed, and sent into a three-stage continuous ball mill for wet ball milling (coarse grinding and fine grinding) to obtain a blank slurry, wherein the mass content of water in the blank slurry is 35%, the specific gravity of the blank slurry is 1.75, the ball outlet flow rate is 93s, the fineness is 1.6% of the mass of the blank slurry remaining on the 325 mesh sieve, and the particle size D50 of the solid particles in the blank slurry is 8.1μm;
[0186] The blank slurry is stored in an underground slurry pool for aging and homogenization for 24 hours, and is sent to a drying tower equipped with 24 spray guns by a blocking pump for powder spraying and granulation, and the blank powder is obtained at the bottom of the spray tower; the particle gradation (standard sieve) of the blank powder is: 20 mesh upper sieve residue ≤0.5wt%, 40 mesh upper sieve residue 70-75wt%, 60 mesh upper sieve residue 15-20wt%, 80 mesh upper sieve residue 3-5wt%, 100 mesh upper sieve residue ≤1wt%, 120 mesh upper sieve residue ≤0.5wt%, the bulk density of the blank powder is 0.95g / mL, and the moisture content of the blank powder is 6.7%; the particles of the blank powder are solid spherical with a relatively smooth surface;
[0187] The green body powder was conveyed to the powder bin by belt for aging for 48 hours (so that the moisture content of the green body powder was 6.2%), and then conveyed to the top hopper of the press, and pressed by SYSTEM frameless belt press at a pressure of 370 bar to obtain a green body (volume density of 1.905 g / cm 3 );
[0188] The green body was transported to a roller kiln for drying at a drying temperature of 155°C and a drying time of 105 minutes, and a body with a strength of 5.2 MPa and a moisture content of less than 0.3% was obtained; the specifications of the obtained body were: length 2.8 m, width 1.0 m, and thickness <4 mm;
[0189] The surface of the green body is physically polished and brushed by a polishing machine to remove impurities on the surface of the dry green body.
[0190] b. Digital white glaze ink decoration
[0191] 62 parts of white glaze powder, 55 parts of isooctyl laurate, 8.9 parts of Huihong HP166, 0.25 parts of BYK306, 0.15 parts of polyamide wax, 0.3 parts of polypropylene glycol 2000, and 0.1 parts of BYK051 were mixed to obtain digital white glaze ink;
[0192] The digital white glaze ink is decorated on the blank by using a digital inkjet machine (the nozzle model is Xaar GS40), and after drying, a base glaze layer is formed.
[0193] c. Pattern decoration
[0194] The pattern is inkjet printed on the base glaze layer. The order of ink colors installed on the inkjet machine is: cyan → purple blue → red brown → dark brown → wrapped red → orange yellow → lemon yellow → green → blue black → red black. The inkjet printing nozzle model is Xaar GS12, forming a pattern decoration layer.
[0195] d. Full glaze decoration
[0196] 420g / m 2 The glaze amount is 100%, and the full-polished glaze slurry is applied to the pattern decoration layer in a pouring glaze manner;
[0197] The semi-finished product is transported to a glaze line dryer for drying, the drying time is 7 minutes, and the drying temperature is 170°C;
[0198] Then it was sent to a firing kiln (the length of the kiln was 300m and the internal width of the kiln was 2.2m) for firing at 1190℃ for 85 minutes to obtain a ceramic rock plate with a specification size of 1000mm×2800mm, a thickness of less than 4mm, and a volume density of 2.6g / cm 3 , the water absorption rate is 0.02%.
[0199] e. Polishing
[0200] The self-developed ceramic rock plate surface polishing processing device (see Chinese invention patent CN215547718U) is used for polishing to obtain a polished glazed ultra-thin ceramic rock plate with a mirror-like gloss effect of 90° and a rupture modulus of 63MPa. The actual picture is as follows Figure 6 shown.
[0201] Example 3
[0202] (1) A method for preparing a full-polished glaze, comprising the steps of:
[0203] By weight, 5 parts of quartz, 2.8 parts of zinc oxide, 15 parts of wollastonite, 31 parts of albite, 13 parts of potassium feldspar, 8 parts of kaolin, 1.2 parts of strontium carbonate, and 7 parts of talc were mixed, and then wet-milled to obtain a slurry (fineness is to pass through a 325-mesh sieve);
[0204] The slurry is then filtered through a 120-mesh sieve to remove iron, and then spray granulated to obtain a powder;
[0205] The powder is put into a sagger, fired at 880° C. for 3 hours, and crushed to obtain the full-polished glaze.
[0206] (2) A method for preparing a full-polished glaze slurry, comprising the steps of:
[0207] By mass, 32 parts of white mineral oil were added to a 1.5T intermittent ball mill cylinder, and then 45 parts of full-polished glaze and 23 parts of frit were gradually added, and finally 1.2 parts of YY502 super dispersant were added for ball milling to obtain a full-polished glaze slurry. The full-polished glaze slurry has a specific gravity of 1.76, a flow rate of 32s, a viscosity of 93mPa·s, and a fineness of passing through a 325 mesh sieve (the residue on the sieve is 0).
[0208] (3) A method for preparing a mirror-polished glazed ultra-thin ceramic rock plate, comprising the steps of:
[0209] a. Preparation of green body:
[0210] By weight, 12 parts of super-plastic ball clay, 18 parts of bentonite, 8 parts of raw kaolin, 17 parts of washed mud, 7 parts of sericite clay, 35 parts of high white potassium feldspar, 3 parts of calcined talc, 9 parts of high sodium high aluminum feldspar powder, 8 parts of α-alumina powder, and 4 parts of composite zirconium powder are mixed, and sent into a three-stage continuous ball mill for ball milling (coarse grinding and fine grinding) to obtain a blank slurry, wherein the mass content of water in the blank slurry is 37%, the specific gravity of the blank slurry is 1.76, the ball outlet flow rate is 88s, the fineness is 1.7% of the mass of the blank slurry remaining on the 325 mesh sieve, and the particle size D50 of the solid particles in the blank slurry is 8.2μm;
[0211] The blank slurry is stored in an underground slurry pool for aging and homogenization for 24 hours, and is sent to a drying tower equipped with 24 spray guns by a blocking pump for powder spraying and granulation, and the blank powder is obtained at the bottom of the spray tower; the particle gradation (standard sieve) of the blank powder is: 20 mesh upper sieve residue ≤0.5wt%, 40 mesh upper sieve residue 70-75wt%, 60 mesh upper sieve residue 15-20wt%, 80 mesh upper sieve residue 3-5wt%, 100 mesh upper sieve residue ≤1wt%, 120 mesh upper sieve residue ≤0.5wt%, the bulk density of the blank powder is 0.97g / mL, and the moisture content of the blank powder is 6.9%; the particles of the blank powder are solid spherical with a relatively smooth surface;
[0212] The green body powder was conveyed to the powder bin by belt for aging for 48 hours (so that the moisture content of the green body powder was 6.3%), and then conveyed to the top hopper of the press, and pressed by SYSTEM frameless belt press at a pressure of 375 bar to obtain a green body (volume density of 1.903 g / cm 3 );
[0213] The green body was transported to a roller kiln for drying at a drying temperature of 145°C and a drying time of 115 minutes, and a body with a strength of 5.3 MPa and a moisture content of less than 0.3% was obtained; the specifications of the obtained body were: length 2.8 m, width 1.0 m, and thickness <4 mm;
[0214] The surface of the green body is physically polished and brushed by a polishing machine to remove impurities on the surface of the dry green body.
[0215] b. Digital white glaze ink decoration
[0216] 60 parts of white glaze powder, 62 parts of isooctyl laurate, 6 parts of Huihong HP166, 0.25 parts of BYK306, 0.15 parts of polyamide wax, 0.3 parts of polypropylene glycol 2000, and 0.1 parts of BYK051 were mixed to obtain digital white glaze ink;
[0217] The digital white glaze ink is decorated on the blank by using a digital inkjet machine (the nozzle model is Xaar GS40), and after drying, a base glaze layer is formed.
[0218] c. Pattern decoration
[0219] The pattern is inkjet printed on the base glaze layer. The order of ink colors installed on the inkjet machine is: cyan → purple blue → red brown → dark brown → wrapped red → orange yellow → lemon yellow → green → blue black → red black. The inkjet printing nozzle model is Xaar GS12, forming a pattern decoration layer.
[0220] d. Full glaze decoration
[0221] 440g / m 2 The glaze amount is 100%, and the full-polished glaze slurry is applied to the pattern decoration layer in a pouring glaze manner;
[0222] The semi-finished product is transported to a glaze line dryer for drying, the drying time is 8 minutes, and the drying temperature is 175°C;
[0223] Then it was sent to a firing kiln (the length of the kiln was 300m and the internal width of the kiln was 2.2m) for firing at 1190℃ for 85 minutes to obtain a ceramic rock plate with a specification size of 1000mm×2800mm, a thickness of less than 4mm, and a volume density of 2.58g / cm 3 , the water absorption rate is 0.021%.
[0224] (5) Polishing
[0225] The self-developed ceramic rock plate surface polishing processing device (see Chinese invention patent CN215547718U) is used for polishing to obtain a polished glazed ultra-thin ceramic rock plate with a mirror soft light effect of 45° glossiness. Its rupture modulus is 57MPa. The actual picture is as follows Figure 7 shown.
[0226] The properties of the mirror-polished glazed ultra-thin ceramic rock slabs in Examples 1-3 are shown in Table 4 below.
[0227] Table 4 Performance of mirror-polished glazed ultra-thin ceramic rock slabs in Examples 1-3
[0228]
[0229] Note: Due to the large flexibility of the ceramic rock slab in the embodiment of the present invention, the test sample size (820mm×100mm) of the elastic limit specified in the national standard for ceramic slabs GB / 23266-2009 cannot detect the specific value of the elastic limit of the product of the present invention; for this reason, when conducting the elastic limit test, the sample size is uniformly changed to 620mm×100mm for testing.
[0230] To summarize, in order to address the problems of cracking, deformation, glaze avoidance, glaze shrinkage, etc. that are caused by the existing traditional glaze water process after ultra-thin rock slab decoration, the glaze decoration process in the present invention is a waterless technology, specifically using full-polished glaze slurry (white mineral oil based) and digital white glaze ink with controllable product deformation, to achieve the preparation of mirror-polished glazed ultra-thin ceramic rock slabs of the present invention.
[0231] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A mirror-polished glazed ultra-thin ceramic rock plate, characterized in that: It comprises a green body, a base glaze layer, a pattern decoration layer and a full-polished glaze layer which are stacked in sequence, wherein the full-polished glaze layer is prepared from a full-polished glaze slurry; The full-polished glaze slurry comprises the following components in parts by mass: 29-35 parts of white mineral oil, 39-50 parts of full-polished glaze, 20-25 parts of frit, 1-1.5 parts of dispersant; The full-polished glaze is prepared from the following raw materials by weight: 3-6 parts of quartz, 2-3.5 parts of zinc oxide, 13-16 parts of wollastonite, 30-33 parts of albite, 10-15 parts of potassium feldspar, 7-9 parts of kaolin, 0.5-2 parts of strontium carbonate, and 6-8 parts of talc; The chemical composition of the frit includes, by mass: SiO2 46-47 parts, Al2O3 26-27 parts, Fe2O3 0-0.1 parts, CaO 17-18 parts, MgO 2.5-3 parts, K2O 2-2.5 parts, Na2O 1-1.5 parts, ZnO 1-2 parts, BaO 0.5-1.0 parts, minus 2.5-3 parts; The raw materials of the green body include, by weight: 10-15 parts of ball clay, 10-25 parts of bentonite, 5-10 parts of kaolin, 15-20 parts of washed mud, 5-10 parts of sericite clay, 30-40 parts of potassium feldspar, 2-4 parts of calcined talc, 7-10 parts of high sodium high aluminum feldspar powder, 6-10 parts of alumina powder, and 3-5 parts of first composite zirconium powder; The base glaze layer is prepared from digital white glaze ink, and the digital white glaze ink comprises the following components in parts by mass: 57-62 parts of white glaze powder, 55-67 parts of organic solvent, 4.9-8.9 parts of first additive, 0.3-1.0 parts of second additive; The white glaze powder comprises the following components: The second composite zirconium powder 85-95 parts, bauxite powder 1-3 parts, potassium feldspar 2-5 parts, fused quartz 2-7 parts; The second composite zirconium powder includes zirconium oxide powder and zirconium silicate powder, or the second composite zirconium powder includes zirconium oxide powder, zirconium silicate powder and aluminum zirconium composite powder; The first auxiliary agent is a dispersant; the second auxiliary agent includes at least one of a leveling agent, a cosolvent, an anti-settling agent, an anti-diffusion agent, and a defoaming agent.
2. The mirror-polished glazed ultra-thin ceramic rock slab according to claim 1 is characterized in that: The dispersant in the full-polishing glaze slurry includes at least one of a polyether dispersant, a polyacrylate dispersant, a polyester dispersant, and a polypropylene hydrocarbon dispersant.
3. A method for preparing the mirror-polished glazed ultra-thin ceramic rock slab according to claim 1, characterized in that: Includes steps: providing a blank; forming a bottom glaze layer on the green body; forming a pattern decoration layer on the base glaze layer; Applying full-polished glaze slurry on the pattern decoration layer, drying, firing, and then polishing to obtain the mirror-polished glazed ultra-thin ceramic rock plate; The preparation method of the full-polished glaze slurry comprises the steps of: By weight, 29 to 35 parts of white mineral oil, 39 to 50 parts of full-polished glaze, 20 to 25 parts of frit, and 1 to 1.5 parts of dispersant are mixed and ball-milled to obtain the full-polished glaze slurry; The preparation method of the full-polished glaze comprises the steps of: Mix 3-6 parts of quartz, 2-3.5 parts of zinc oxide, 13-16 parts of wollastonite, 30-33 parts of albite, 10-15 parts of potassium feldspar, 7-9 parts of kaolin, 0.5-2 parts of strontium carbonate and 6-8 parts of talc by weight, and then perform wet ball milling, iron removal and spray granulation in sequence to obtain a powder; The powder is calcined at a temperature of 850-950° C. for 2-4 hours and crushed to obtain the full-polished glaze.
Citation Information
Patent Citations
Ceramic rock plate surface polishing device and polishing machine
CN215547718U
Low temperature ceramic inkjet ink
CN103642317A
Ceramic sheet ink-jet underglaze decorative glaze, preparation method thereof and ceramic sheet
CN112358188A
Ultra-flat glaze for ceramic tile, ceramic tile and manufacturing method of ceramic tile
CN112429967A
3mm glaze decorated fully-polished ceramic rock plate with light-transmitting effect and manufacturing method of 3mm glaze decorated fully-polished ceramic rock plate