A high crystallinity divalent europium doped barium chloride nanocrystalline glass and preparation method thereof
By adding specific components to the scintillation crystal glass and using graphite powder reduction method, the problems of water resistance stability and Eu valence control of traditional scintillation crystal glass are solved, and high crystallinity and low-cost divalent europium doped chlorine are achieved. Barium nanocrystalline glass significantly improves the performance of scintillator detectors.
Patent Information
- Application Number
- CN202310887028.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-07-19
AI Technical Summary
Traditional scintillation crystal glass has shortcomings in water resistance stability and Eu valence control, and it is difficult to meet the requirements of high crystallinity and low cost, which limits its application in scintillator detectors.
Using high-resolution crystalline divalent europium-doped barium chloride nanocrystalline glass, the appropriate amount of AlF3, CaF2, SrF2, YF3 and Al(PO3)3 are added to the glass phase, combined with graphite powder reduction method and segmented high-temperature melting process. A nanocrystalline glass with high light transmission and stability is formed to ensure that BaCl2 is charged and analyzed and volatilized.
It achieves high crystallinity, good light transmittance and luminous performance, significantly improves the water resistance and radiation stability of the glass, and has significantly higher scintillation intensity than commercial BGO single crystals, and is suitable for efficient X-ray imaging and electron microscope detectors.
Smart Images

Figure CN116813208B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanocrystalline glass, and in particular relates to a high-crystallization divalent europium-doped barium chloride nanocrystalline glass and a preparation method thereof. Background Art
[0002] Scintillators are a type of luminescent material that can absorb high-energy particles (such as X-rays, gamma rays, etc.) and convert them into low-energy photons (visible light, ultraviolet light, etc.). Scintillators, as core components, are combined with devices such as photomultiplier tubes to form scintillator detectors, which have the advantages of high detection efficiency, short resolution time, and ease of use. Therefore, they can be widely used in medical imaging, industrial monitoring, homeland security, geological exploration, scientific research and other fields.
[0003] Scintillators can be divided into inorganic scintillators and organic scintillators. Organic scintillators have a short luminescence decay time, but low light yield, while inorganic scintillators have high light yield, good linearity, and wider applicability.
[0004] Inorganic scintillators can be divided into oxides and halides. 2+ The non-fluorine halide crystals of scintillation-activated ions exhibit excellent scintillation properties such as light output and energy resolution. This is due to the heavy atomic number of the halide crystal and the divalent Eu 2+ The fd transition is a permitted transition determined by the spectral selection law and has high luminescence efficiency. However, non-fluorine halide crystals always face problems such as easy deliquesce, difficulty in large-scale growth, and long preparation cycle.
[0005] Precipitating halide scintillating nanocrystals in glass to obtain transparent glass-ceramic scintillators can avoid the above problems, while reducing the high cost of high-purity materials and harsh single crystal preparation conditions, and maintaining the advantages of high transmittance and easy processing. However, the solubility of halides in oxide glass is low, and the high melting temperature makes halides easily volatilize. The final residual halide content in the glass is low, which limits the degree of halide crystallization after heat treatment of the glass.
[0006] Classic fluorozirconate glass was first used to precipitate Eu due to its good glass-forming properties. 2+ Glass matrix of doped halide nanocrystals.
[0007] A Chinese patent with publication number CN1927752A discloses an infrared-transparent fluorozirconate glass-ceramic and a preparation method thereof, which is characterized in that LaF3 is added to the ZrF4-BaF2-YF3-AlF3 fluoride glass component, and the molar percentage composition range of the glass-ceramic is: ZrF4: 50-55, BaF2: 15-33, YF3: 10-22, AlF3: 3-7, LaF3: 2-8. The preparation method is to first prepare the fluorozirconate glass by a melting method, and then, through precision heat treatment, heat-treat the base glass to microcrystallize and obtain transparent fluorozirconate glass-ceramic. However, the fluorozirconate glass-ceramic prepared by the above patent has poor water resistance and stability, and the valence state of Eu is uncontrollable (it is easy to react with Zr 4+ The redox reaction occurs during the crystallization and non-luminescent impurity phase is easily precipitated, which limits its further development and industrial application.
[0008] Currently, scintillator detectors are developing towards higher detection efficiency, higher imaging resolution, lower cost, larger area and higher long-term stability. Traditional scintillator microcrystalline (nanocrystalline) glass is difficult to meet such requirements, so it is necessary to develop new types of scintillator detectors containing high crystallinity Eu. 2+ Doped halide nanocrystals, transparent high-crystallinity nanocrystalline glass scintillators with good stability and low cost meet such development needs. Summary of the invention
[0009] The invention provides a high-crystallization divalent europium-doped barium chloride nanocrystalline glass with high light transmittance, good luminescence performance and high stability.
[0010] A specific embodiment of the present invention provides a high crystallinity divalent europium-doped barium chloride nanocrystalline glass, comprising a crystal phase and a glass phase, wherein the volume fraction (crystallization degree) of the crystal phase is 15-40%, and the volume fraction of the glass phase is 60-85%;
[0011] The crystalline phase comprises the following components in percentage by mass, including: 80-99% BaCl2, 1-20% EuX, where X is a halogen element;
[0012] The glass phase contains the following components in percentage by mass, including: 25-40% AlF3, 10-15% CaF2, 8-15% SrF2, 0-20% BaF2, 15-25% YF3, and 5-20% Al(PO3)3.
[0013] Since the glass phase provided by the present invention has good solubility for the components of the crystalline phase and the melting point of the glass phase provided by the present invention is low, the volatilization of the crystalline phase elements can be avoided during the preparation process. Therefore, a larger volume fraction of the crystalline phase can be precipitated, so that the high-crystallization divalent europium-doped barium chloride nanocrystalline glass has good light transmittance and high luminescence performance.
[0014] The crystalline phase provided by the present invention has enough BaCl2, so it can absorb more light energy and transfer the absorbed energy to the Eu element, thereby achieving better luminescence performance.
[0015] The components of the glass phase provided by the present invention are mainly Al and F elements, and provide a suitable component ratio, so that the high-crystallization divalent europium-doped barium chloride nanocrystalline glass still has high light transmittance and luminescence performance, that is, high stability, after long-term use in a high humidity environment.
[0016] Furthermore, the volume fraction of the crystal phase is 25-30%, and the volume fraction of the glass phase is 70-75%. Under the appropriate volume fractions of the crystal phase and the glass phase, the visible light transmittance of the high-crystallization divalent europium-doped barium chloride nanocrystalline glass obtained is 88-95%, and the luminous intensity of the scintillation is 200-250% of that of BGO.
[0017] Furthermore, X is Cl element. EuCl3 and BaCl2 are both chlorides, which are conducive to the formation of Ba, Eu and Cl phase separation in the precursor glass, providing a structural basis for the subsequent formation of BaCl2:Eu nanocrystals.
[0018] Furthermore, the BaCl2 is 90-95% and the EuX is 5-10%. At this concentration, the luminescent ions are more, and strong self-absorption and scintillation luminescence quenching will not be caused due to excessive concentration. At this doping concentration, and when the crystal phase volume is 35-40% and the glass phase volume is 60-65%, the europium-doped barium chloride nanocrystalline glass obtained has a scintillation luminescence intensity of 300%-350% of BGO.
[0019] The present invention also provides a method for preparing divalent europium-doped barium chloride nanocrystalline glass with high crystallinity, comprising:
[0020] (1) preparing, grinding and mixing the components of the europium-doped barium chloride nanocrystalline glass in accordance with their mass percentages to obtain a powder raw material;
[0021] (2) placing the powder raw material obtained in step (1) into a small-capacity crucible, placing the small-capacity crucible into a large-capacity crucible with graphite powder at the bottom, covering the large-capacity crucible with a graphite cover, and then firing the large-capacity crucible;
[0022] (3) After firing, the glass liquid in the small-capacity crucible is poured onto a preheated metal plate and then pressed into shape to obtain shaped glass;
[0023] (4) heating the formed glass obtained in step (3) to 400-430° C. and keeping the temperature for 120-180 min, and cooling the furnace to room temperature to obtain a precursor glass;
[0024] (5) Heat treating the precursor glass to obtain divalent europium-doped barium chloride nanocrystalline glass with high crystallinity, wherein the heat treatment process is as follows: heating from room temperature to 460-480°C at a rate of 5-10°C / min and keeping the temperature for 2-6 hours, then heating to 500-520°C at a rate of 0.2-2°C / min and keeping the temperature for 10-150 minutes.
[0025] The present invention uses a double crucible method and increases the temperature to make the bottom graphite powder and the top graphite cover generate carbon monoxide gas, and the trivalent europium element is reduced by the carbon monoxide gas, and the trivalent europium element is converted into a divalent europium element. The divalent europium element obtained after the reduction is more likely to replace part of the Ba element in the BaCl2 nanocrystal with the same valence in the subsequent heat treatment process, so as to prepare for the subsequent realization of the luminescent crystal phase.
[0026] Since the crystallization of BaCl2 in fluoroaluminum-phosphorus glass is very sensitive to temperature, when the precursor glass is heat-treated, the present invention heats the glass to a suitable temperature at a low speed, i.e., 0.2-2°C / min, thereby avoiding the uneven size of BaCl2 grains. Large grains can produce scattering, thereby reducing the transmittance of europium-doped barium chloride nanocrystalline glass.
[0027] Furthermore, in step (2), the amount of the graphite powder accounts for 20%-40% of the capacity of the large-capacity crucible.
[0028] Furthermore, in step (2), the firing process is: keeping the temperature at 1100-1200°C for 25-30 minutes, cooling to 950-1000°C and keeping for 3-5 minutes. Since the melting point of the phosphate in the glass phase provided by the present invention is relatively high, the melting temperature is set at 1100-1200°C. In order to make the molten glass liquid have a certain viscosity to facilitate subsequent molding, make the casting molding process more controllable, and obtain a highly transparent precursor glass, the present invention lowers the firing temperature to a suitable temperature.
[0029] Furthermore, the material of the metal plate is Cu, Al and Fe.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The large amount of fluoride composition in the glass of the present invention can ensure that the glass melting temperature is low, so that less barium chloride is volatilized during the glass melting process, so that the nanocrystalline glass provided by the present invention has a higher barium chloride nanocrystal crystallization degree, and thus has higher luminescence characteristics; and because the addition of metaphosphate Al(PO3)3 can improve the glass forming ability and thermal stability, the nanocrystalline glass provided by the present invention has high transmittance, good water resistance and radiation stability.
[0032] The graphite powder reduction method of the present invention has a very good effect. In the ultraviolet excited fluorescence spectrum, Eu 3+ The luminescence peak is invisible and has a high photoluminescence quantum efficiency. In the spectrum of X-ray excitation, Eu 2+ The luminescence intensity is much higher than Eu 3+ The luminescent and blinking light output is significantly higher than that of commercial BGO single crystals.
[0033] The present invention can increase the high-temperature viscosity of the molten glass liquid through a segmented high-temperature melting process, make the casting and molding process more controllable, and obtain a highly transparent precursor glass; the segmented heat treatment process can controllably precipitate BaCl2 nanocrystals with high crystallinity and adjustable size. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a UV-visible transmission spectrum of the high-crystallization divalent europium-doped barium chloride nanocrystalline glass prepared in Example 1 of the present invention;
[0035] Figure 2 This is an X-ray diffraction spectrum of the high crystallinity divalent europium doped barium chloride nanocrystalline glass prepared in Example 1 of the present invention;
[0036] Figure 3 This is an excitation emission fluorescence spectrum of the high crystallinity divalent europium doped barium chloride nanocrystalline glass prepared in Example 1 of the present invention;
[0037] Figure 4 This is a scintillation fluorescence emission spectrum of the high crystallinity divalent europium-doped barium chloride nanocrystalline glass under X-ray excitation prepared in Example 1 of the present invention;
[0038] Figure 5 This is a photo of the high crystallinity divalent europium-doped barium chloride nanocrystalline glass prepared in Example 1 of the present invention;
[0039] Figure 6 This is a transmission electron microscope image of the high crystallinity divalent europium doped barium chloride nanocrystalline glass prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the following describes the embodiments and comparative examples in detail in conjunction with the accompanying drawings.
[0041] Example 1
[0042] (1) Weigh 15 g of the required mass of powder raw materials according to the mass ratio of AlF3:CaF2:SrF2:BaF2:YF3:Al(PO3)3:BaCl2:EuF3=26:9:5:7:15:11:25:2, grind them thoroughly and mix them evenly.
[0043] (2) The powder raw material is placed in a small corundum crucible, and then the small corundum crucible is placed in a large corundum crucible with graphite powder about 30% of the capacity of the large crucible at the bottom. The large corundum crucible is then covered with a graphite cover plate and placed in an electric furnace at 1130°C for insulation melting for 25 minutes, and then the temperature is reduced to 970°C and maintained for 5 minutes.
[0044] (3) The graphite cover on the large corundum crucible is removed, and after the small crucible is removed from the large crucible, molten glass with a suitable viscosity is quickly poured onto a preheated copper plate, and then quickly pressed into shape with another preheated copper plate.
[0045] (4) The glass is quickly transferred to a furnace at 420°C and kept warm for 120 minutes, and then cooled to room temperature along with the furnace to obtain a precursor glass.
[0046] (5) Heat treatment crystallization: The precursor glass is placed in a furnace and first heated from room temperature to 460°C at a rate of 5°C / min and kept at this temperature for 4 hours, then heated to 510°C at a rate of 2°C / min and kept at this temperature for 10 minutes, and then cooled to room temperature in the furnace to obtain nanocrystalline glass. Figure 5 shown.
[0047] The prepared nanocrystalline glass was tested after grinding and polishing, and the UV-visible transmission spectrum of the glass was measured. Figure 1 As shown, the transmittance at 600 nm is 93%.
[0048] The X-ray diffraction pattern of the nanocrystalline glass shows that the BaCl2 crystal phase has a strong diffraction peak and no other impurities in the glass. The crystallization fraction is calculated to be 28%.
[0049] like Figure 3 As shown, the excitation emission spectrum of the photoluminescence of the nanocrystalline glass was measured, with an excitation peak wavelength of 373 nm and an emission peak wavelength of 402 nm.
[0050] The scintillation luminescence spectrum of nanocrystalline glass under X-ray excitation was measured, and the integrated intensity of the scintillation luminescence can reach 212% of that of commercial scintillating single crystal BGO. In summary, by preparing highly crystallized divalent europium-doped BaCl2 nanocrystalline glass scintillators, they can be used for X-ray imaging and electron microscope detectors.
[0051] After the BaCl2 nanocrystalline glass was placed in distilled water for 96 hours and then taken out, there was no obvious change in the transmittance and scintillation luminescence properties.
[0052] like Figure 6 As shown, the BaCl2 nanocrystals are evenly distributed in the fluoroaluminum-phosphorus glass.
[0053] Example 2
[0054] (1) Weigh 15 g of the required mass of powder raw materials according to the mass ratio of AlF3:CaF2:SrF2:BaF2:YF3:Al(PO3)3:BaCl2:EuF3=25:9:6:9:15:11:23:2, grind them thoroughly and mix them evenly;
[0055] (2) placing the powder raw material into a small corundum crucible, and then placing the small corundum crucible into a large corundum crucible with graphite powder about 20% of the capacity of the large crucible at the bottom, and then covering the large corundum crucible with a graphite cover plate and placing it in an electric furnace at 1100° C. for 25 minutes, and then cooling to 950° C. and maintaining for 3 minutes;
[0056] (3) The graphite cover on the large corundum crucible is removed, and after the small crucible is removed from the large crucible, molten glass with a suitable viscosity is quickly poured onto a preheated copper plate, and then quickly pressed into shape with another preheated copper plate;
[0057] (4) The glass is quickly transferred to a furnace at 420° C. and kept warm for 120 minutes, and then cooled to room temperature along with the furnace to obtain a precursor glass;
[0058] (5) Heat treatment for crystallization: The precursor glass is placed in a furnace and first heated from room temperature to 460°C at a rate of 5°C / min and kept at this temperature for 2 hours. Then, the temperature is heated to 500°C at a rate of 1°C / min and kept at this temperature for 10 minutes. Then, the glass is cooled to room temperature in the furnace to obtain nanocrystalline glass.
[0059] The prepared nanocrystalline glass was tested after being ground and polished, and the ultraviolet-visible transmission spectrum of the glass was measured, and the transmittance at 600 nanometers was 87%.
[0060] The X-ray diffraction pattern of the nanocrystalline glass shows that the BaCl2 crystal phase has a strong diffraction peak and no other impurities in the glass. The crystallization fraction is calculated to be 31%.
[0061] The excitation emission spectra of the photoluminescence of the nanocrystalline glass were measured, and the excitation peak wavelength was 373nm, and the emission peak wavelength was 403nm.
[0062] The scintillation luminescence spectrum of nanocrystalline glass under X-ray excitation was measured, and the integrated intensity of the scintillation luminescence can reach 150% of that of commercial scintillating single crystal BGO. In summary, by preparing highly crystallized divalent europium-doped BaCl2 nanocrystalline glass scintillators, they can be used for X-ray imaging and electron microscope detectors.
[0063] Example 3
[0064] (1) Weigh 15 g of the required mass of powder raw materials according to the mass ratio of AlF3:CaF2:SrF2:BaF2:YF3:Al(PO3)3:BaCl2:EuF3=29:9:6:8:15:7:24:2, grind them thoroughly and mix them evenly;
[0065] (2) placing the powder raw material into a small corundum crucible, and then placing the small corundum crucible into a large corundum crucible with graphite powder about 25% of the capacity of the large crucible at the bottom, and then covering the large corundum crucible with a graphite cover plate and placing it in an electric furnace at 1150° C. for 27 minutes, and then cooling to 98° C. and maintaining for 5 minutes;
[0066] (3) The graphite cover on the large corundum crucible is removed, and after the small crucible is removed from the large crucible, molten glass with a suitable viscosity is quickly poured onto a preheated copper plate, and then quickly pressed into shape with another preheated copper plate;
[0067] (4) The glass is quickly transferred to a furnace at 420° C. and kept warm for 120 minutes, and then cooled to room temperature along with the furnace to obtain a precursor glass;
[0068] (5) Heat treatment for crystallization: The precursor glass is placed in a furnace and first heated from room temperature to 470°C at a rate of 8°C / min and kept at this temperature for 4 hours. Then, the temperature is heated to 510°C at a rate of 2°C / min and kept at this temperature for 10 minutes. Then, the furnace is cooled to room temperature to obtain nanocrystalline glass.
[0069] The prepared nanocrystalline glass was tested after being ground and polished, and the UV-visible transmission spectrum of the glass was measured, and the transmittance at 600 nanometers was 88%.
[0070] The X-ray diffraction pattern of the nanocrystalline glass shows that the BaCl2 crystal phase has a strong diffraction peak and no other impurities in the glass. The calculated crystallization fraction is 29%.
[0071] The excitation emission spectra of the photoluminescence of the nanocrystalline glass were measured, and the excitation peak wavelength was 371nm and the emission peak wavelength was 403nm.
[0072] The scintillation spectrum of nanocrystalline glass under X-ray excitation was measured, and the integrated intensity of the scintillation luminescence can reach 162% of that of commercial scintillating single crystal BGO. In summary, by preparing highly crystallized divalent europium-doped BaCl2 nanocrystalline glass scintillators, they can be used for X-ray imaging and electron microscope detectors.
[0073] Example 4
[0074] (1) Weigh 15 g of the required mass of powder raw materials according to the mass ratio of AlF3:CaF2:SrF2:BaF2:YF3:Al(PO3)3:BaCl2:EuF3=26:9:5:2:17:10:33:3, grind them thoroughly and mix them evenly;
[0075] (2) placing the powder raw material into a small corundum crucible, and then placing the small corundum crucible into a large corundum crucible with graphite powder about 40% of the capacity of the large crucible at the bottom, and then covering the large corundum crucible with a graphite cover plate and placing it in an electric furnace at 1150° C. for 25 minutes, and then cooling to 95° C. and maintaining for 4 minutes;
[0076] (3) The graphite cover on the large corundum crucible is removed, and after the small crucible is removed from the large crucible, molten glass with a suitable viscosity is quickly poured onto a preheated copper plate, and then quickly pressed into shape with another preheated copper plate;
[0077] (4) The glass is quickly transferred to a furnace at 420° C. and kept warm for 120 minutes, and then cooled to room temperature along with the furnace to obtain a precursor glass;
[0078] (5) Heat treatment for crystallization: The precursor glass is placed in a furnace and first heated from room temperature to 460°C at a rate of 7°C / min and kept at this temperature for 5 hours. Then, the temperature is heated to 510°C at a rate of 2°C / min and kept at this temperature for 60 minutes. Then, the glass is cooled to room temperature in the furnace to obtain microcrystalline glass.
[0079] The prepared nanocrystalline glass was tested after being ground and polished, and the UV-visible transmission spectrum of the glass was measured, and the transmittance at 600 nanometers was 60%.
[0080] The X-ray diffraction spectrum of nanocrystalline glass shows that BaCl2 crystal phase has strong diffraction peaks and no other impurities in the glass. The crystallization fraction is calculated to be 37%. Figure 2 shown.
[0081] The excitation emission spectra of the photoluminescence of the nanocrystalline glass were measured, and the excitation peak wavelength was 375nm, and the emission peak wavelength was 399nm.
[0082] The scintillation luminescence spectrum of nanocrystalline glass under X-ray excitation is measured, and the integrated intensity of the scintillation luminescence can reach 312% of that of commercial scintillation single crystal BGO, such as Figure 4 In summary, by preparing the high crystallinity divalent europium-doped BaCl2 nanocrystalline glass scintillator, it can be used for X-ray imaging and electron microscope detectors.
[0083] Example 5
[0084] (1) Weigh 15 g of the required mass of powder raw materials according to the mass ratio of AlF3:CaF2:SrF2:BaF2:YF3:Al(PO3)3:BaCl2:EuF3=23:9:5:4:17:18:23:1, grind them thoroughly and mix them evenly;
[0085] (2) placing the powder raw material into a small corundum crucible, and then placing the small corundum crucible into a large corundum crucible with graphite powder about 30% of the capacity of the large crucible at the bottom, and then covering the large corundum crucible with a graphite cover plate and placing it in an electric furnace at 1150° C. for 30 minutes of heat preservation, and then cooling to 1000° C. and maintaining for 5 minutes;
[0086] (3) The graphite cover on the large corundum crucible is removed, and after the small crucible is removed from the large crucible, molten glass with a suitable viscosity is quickly poured onto a preheated copper plate, and then quickly pressed into shape with another preheated copper plate;
[0087] (4) The glass is quickly transferred to a furnace at 420° C. and kept warm for 120 minutes, and then cooled to room temperature along with the furnace to obtain a precursor glass;
[0088] (5) Heat treatment for crystallization: The precursor glass is placed in a furnace and first heated from room temperature to 480°C at a rate of 10°C / min and kept at this temperature for 6 hours. Then, the temperature is heated to 520°C at a rate of 3°C / min and kept at this temperature for 120 minutes. Then, the glass is cooled to room temperature in the furnace to obtain microcrystalline glass.
[0089] The prepared nanocrystalline glass was tested after being ground and polished, and the ultraviolet-visible transmission spectrum of the glass was measured, and the transmittance at 600 nanometers was 92%.
[0090] The X-ray diffraction spectrum of the nanocrystalline glass shows that the BaCl2 crystal phase has a strong diffraction peak and no other impurities in the glass. The crystallization fraction is calculated to be 18%.
[0091] The excitation emission spectra of the photoluminescence of the nanocrystalline glass were measured, and the excitation peak wavelength was 370nm, and the emission peak wavelength was 405nm.
[0092] The scintillation luminescence spectrum of nanocrystalline glass under X-ray excitation was measured, and the integrated intensity of the scintillation luminescence can reach 106% of that of commercial scintillating single crystal BGO. In summary, by preparing highly crystallized divalent europium-doped BaCl2 nanocrystalline glass scintillators, they can be used for X-ray imaging and electron microscope detectors.
[0093] The above embodiments are used to illustrate the present invention rather than to limit the present invention. Any modification and change made to the present invention within the spirit of the present invention and the protection scope of the claims shall fall within the protection scope of the present invention.
Claims
1. A high crystallinity divalent europium doped barium chloride nanocrystalline glass, characterized in that: It comprises a crystal phase and a glass phase, wherein the volume fraction of the crystal phase is 15-40%, and the volume fraction of the glass phase is 60-85%; The crystalline phase comprises the following components in percentage by mass, including: 80-99% BaCl2, 1-20% EuX, where X is a halogen element; The glass phase contains the following components in percentage by mass, including: 25-40% AlF3, 10-15% CaF2, 8-15% SrF2, 0-20% BaF2, 15-25% YF3, and 5-20% Al(PO3)3.
2. The high crystallinity divalent europium doped barium chloride nanocrystalline glass according to claim 1, characterized in that: The volume fraction of the crystal phase is 25-30%, and the volume fraction of the glass phase is 70-75%.
3. The high crystallinity divalent europium-doped barium chloride nanocrystalline glass according to claim 1, characterized in that: The X is a Cl element.
4. The high crystallinity divalent europium doped barium chloride nanocrystalline glass according to claim 1, characterized in that: The crystalline phase comprises the following components in percentage by mass: BaCl2 is 90-95% and EuX is 5-10%.
5. A method for preparing divalent europium doped barium chloride nanocrystalline glass with high crystallinity according to any one of claims 1 to 4, characterized in that: include: (1) preparing, grinding and mixing the components of the high crystallinity divalent europium-doped barium chloride nanocrystalline glass according to any one of claims 1 to 4 in accordance with their mass percentages to obtain a powder raw material; (2) placing the powder raw material obtained in step (1) into a small-capacity crucible, placing the small-capacity crucible into a large-capacity crucible with graphite powder at the bottom, covering the large-capacity crucible with a graphite cover, and then firing the large-capacity crucible; (3) After firing, the glass liquid in the small-capacity crucible is poured onto a preheated metal plate and then pressed into shape to obtain shaped glass; (4) heating the formed glass obtained in step (3) to 400-430° C. and keeping the temperature for 120-180 min, and cooling the furnace to room temperature to obtain a precursor glass; (5) Heat treating the precursor glass to obtain divalent europium-doped barium chloride nanocrystalline glass with high crystallinity, wherein the heat treatment process is as follows: heating from room temperature to 460-480°C at a rate of 5-10°C / min and keeping the temperature for 2-6 hours, then heating to 500-520°C at a rate of 0.2-2°C / min and keeping the temperature for 10-150 minutes.
6. The method for preparing the high crystallinity divalent europium-doped barium chloride nanocrystalline glass according to claim 5, characterized in that: In step (2), the amount of the graphite powder accounts for 20%-40% of the capacity of the large-capacity crucible.
7. The method for preparing divalent europium-doped barium chloride nanocrystalline glass with high crystallinity according to claim 5, characterized in that: In step (2), the firing process conditions are: keeping at 1100-1200°C for 25-30 minutes, cooling to 950-1000°C and keeping for 3-5 minutes.
8. The method for preparing divalent europium-doped barium chloride nanocrystalline glass with high crystallinity according to claim 5, characterized in that: The metal plate material is one of Cu, Al or Fe.