A matte deep copper-nickel salt colored aluminum profile and preparation method thereof

By optimizing the raw material formula and preparation process of aluminum alloy, the color difference and uneven coloring problems in the production of extinct bronze aluminum profiles are solved, and the uniformity of the dark bronze base color and high-quality surface are achieved, which improves the coloring effect of nickel salt.

CN116815269BActive Publication Date: 2024-12-03GUANGDONG WEIYE ALUMINUM FACTORY GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310407913.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-12-03
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

The production control of high-quality extinct bronze and aluminum profiles is difficult to control, and the color difference is high sensitivity. The residual acid water in the oxide film pores during the nickel salt coloring process leads to uneven coloring, and the low dispersion of nickel ion affects the uniformity of coloring.

Method used

By optimizing the formulation and preparation process of aluminum alloy raw materials, including homogenization treatment, sandblasting treatment, anodization treatment and electrolytic chromatography, the pH and temperature of the electrolyte are controlled, and process parameters are adjusted to improve color uniformity and color quality.

Benefits of technology

The dark bronze coloring effect is improved, the color defects at both ends are eliminated, the color uniformity and surface quality of the aluminum profile are ensured, the generation of β-FeSiAl phase is reduced, and the rosiness and gloss of the tinting background are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004182151610000141
    Figure BDA0004182151610000141
  • Figure BDA0004182151610000142
    Figure BDA0004182151610000142
  • Figure BDA0004182151610000143
    Figure BDA0004182151610000143
Patent Text Reader

Abstract

The invention discloses a matte deep bronze nickel salt colored aluminum profile and a preparation method thereof. The aluminum profile comprises the following components by mass percentage: Mg≤0.9%, Si≤0.6%, Fe≤0.2%, Cu≤0.1%, Mn≤0.05%, Ti≤0.05%, Cr≤0.05%, Zn≤0.05%, and the balance is Al and inevitable impurities; the preparation process comprises: smelting casting, homogenization, extrusion quenching, pretreatment, anodizing, electrolytic coloring and matte photophoresis. The invention improves the coloring effect of the profile by optimizing the formula and coordinating a specific preparation process, and the obtained profile has a deep bronze base color with a ruddy color and uniform color.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy materials, and in particular to a matte deep bronze nickel salt colored aluminum profile and a preparation method thereof. Background Art

[0002] At present, high-quality matte bronze aluminum profiles are very popular in the market, especially in high-end decoration, villa projects, high-end garage shutters and other scenes. They are moist and translucent, with strong color, and combined with porcelain, they feel silky and high-end. However, the production control of high-quality matte bronze aluminum profiles is very challenging. The surface color quality is difficult to control, the color difference is highly sensitive, and the quality requirements of the previous process materials are strict.

[0003] The main coloring method for matte bronze aluminum profiles is electrolytic coloring. The electrolytic coloring methods mainly include nickel salt coloring, tin salt coloring, and nickel-tin mixed salt coloring. The effect of nickel salt coloring is more ideal, and the color is visually rich and textured. From the colorimeter data analysis, the color performance associated with the red value and brightness is good, and it has a very leading advantage in drug consumption and coloring efficiency.

[0004] However, the single nickel salt coloring series products have more stringent requirements on the quality of raw materials and production process control. The coloring characteristics of nickel salts are relatively sensitive, and the pH value of the bath solution is lower. Therefore, during the production process, if there is a lot of residual acid water in the oxide film pores, it will cause coloring hydrogen reduction, resulting in color fluctuations and uneven coloring. In addition, the nickel salt itself has a low dispersion of metal nickel ions under the action of the coloring electric field. Combined with the circulation volume of the bath solution and the influence of monovalent cationic impurities, it will aggravate the impact on coloring uniformity and color effect. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a matte deep bronze nickel salt colored aluminum profile and a preparation method thereof, and the coloring effect of the profile is improved by optimizing the formula and coordinating a specific preparation process, and the obtained profile has a good deep bronze coloring effect and uniform color.

[0006] In order to solve the above technical problems, the embodiment of the present invention provides a matte dark bronze nickel salt colored aluminum profile and a preparation method thereof, comprising the following steps:

[0007] (1) melting and casting the raw materials according to the formula to obtain aluminum alloy cast rods, and homogenizing the raw materials, wherein the raw materials are composed of the following components by mass percentage: Mg≤0.9%, Si≤0.6%, Fe≤0.2%, Cu≤0.1%, Mn≤0.05%, Ti≤0.05%, Cr≤0.05%, Zn≤0.05%, and the balance is Al and unavoidable impurities, with a single impurity of ≤0.05% and a total impurity of ≤0.15%;

[0008] (2) extruding the aluminum alloy cast rod after homogenization treatment to obtain an aluminum profile blank, and quenching the blank; the upper machine temperature of the aluminum alloy cast rod after homogenization treatment is lower than the upper machine temperature of the mold;

[0009] (3) sandblasting the aluminum profile blank after quenching;

[0010] (4) pre-treating the aluminum profile blank after sandblasting;

[0011] (5) subjecting the pretreated aluminum profile blank to anodizing treatment and performing a first water washing treatment;

[0012] (6) immersing the aluminum profile blank after the first water washing treatment into an electrolyte, performing an electrolytic coloring treatment, and performing a second water washing treatment;

[0013] The electrolyte comprises the following components: nickel sulfate at a concentration of 135-150 g / L, boric acid at a concentration of 38-42 g / L, and monovalent cations at a concentration of ≤10 ppm;

[0014] (7) The aluminum profile blank after the second water washing treatment is subjected to matte photophoresis treatment and cured.

[0015] As an improvement of the above scheme, the aluminum profile is composed of the following components by mass percentage: Mg 0.48-0.53%, Si 0.38-0.41%, Fe 0.01-0.15%, Cu 0.01-0.1%, Mn 0.01-0.05%, Ti 0.01-0.05%, Cr 0.01-0.05%, Zn 0.01-0.05%, and the balance is Al and unavoidable impurities, with a single impurity of 0.01-0.05% and a total amount of 0.01-0.15%.

[0016] As an improvement of the above scheme, in step (2), the upper machine temperature of the aluminum alloy casting rod is 465-475°C, and the upper machine temperature of the mold is 475-485°C;

[0017] The quenching treatment is a strong wind quenching treatment.

[0018] As an improvement of the above scheme, in step (6), the pH of the electrolyte is 3.8-4.5, the temperature of the electrolytic cell is 24-26° C., and the electrolytic coloring time is 225-310 s;

[0019] The second water washing treatment lasts for 1-10 seconds.

[0020] As an improvement of the above scheme, in step (1), the temperature of the homogenization treatment is 540℃-560℃, and the time of the homogenization treatment is ≥3.5h; after the homogenization treatment is completed, the aluminum alloy casting rod is cooled by strong wind for 4-6h until the rod temperature is 200-210℃, and then cooled to room temperature by water mist.

[0021] As an improvement of the above scheme, in step (4), the pretreatment includes degreasing treatment, alkaline etching treatment and neutralization treatment in sequence.

[0022] The degreasing liquid used in the degreasing treatment has a degreasing component concentration of 60-70 g / L, and the degreasing treatment time is 1-3 min;

[0023] The alkali concentration in the alkali etching solution used in the alkali etching treatment is 90-130 g / L, the alkali etching treatment time is 1-3 min, and the alkali etching temperature is 45-55° C.

[0024] The neutralization liquid used in the neutralization treatment is a sulfuric acid solution, the concentration of free sulfuric acid in the sulfuric acid solution is 180-200 g / L, and the neutralization treatment time is 0.5-2 min.

[0025] As an improvement of the above scheme, in step (5), the pretreated aluminum profile blank is immersed in an anodizing treatment solution and energized, the sulfuric acid concentration in the anodizing treatment solution is 220-280 g / L, the aluminum ion concentration is 10-20 g / L, and the current density during the anodizing treatment is 120-140 A / m 2 , the oxidation tank temperature is 18-20℃, and the oxidation time is 20-30min;

[0026] The first water washing treatment includes a first water washing treatment, a second water washing treatment and a third water washing treatment;

[0027] The pH of the washing liquid in the first washing treatment is 0.8-1.7, the washing time is 20-30s, and the conductivity of the washing liquid is ≤15μS / cm;

[0028] The pH of the washing liquid in the second washing treatment is 2.1-3.7, the washing time is 20-30s, and the conductivity of the washing liquid is ≤15μS / cm;

[0029] The pH of the washing liquid in the third washing treatment is 4.0-5.0, the washing time is 20-30s, and the conductivity of the washing liquid is ≤15μS / cm.

[0030] As an improvement of the above scheme, in step (7), the aluminum profile blank after the second water washing treatment is immersed in an electrophoresis solution for extinction electrophoresis treatment, wherein the pH of the electrophoresis solution is 8.3-8.6, the conductivity is 650-950 μS / cm, the solid content is 9.5-10.5wt%, the electrophoresis temperature is 18-22° C., and the electrophoresis voltage is 120-150V;

[0031] After the matting photophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting photophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing;

[0032] The conductivity of the washing liquid of the RO1 washing tank is ≤250μS / cm, the solid content is 0.3-1.5wt%, and the pH is 8.5-9.5;

[0033] The conductivity of the washing liquid of the RO2 washing tank is ≤125μS / cm, the solid content is 0.1-0.2wt%, and the pH is 8.5-9.5;

[0034] The aluminum profile blank after the third water washing treatment is cured at a temperature of 180-190° C. and a curing time of 40-50 minutes.

[0035] Implementing the embodiments of the present invention has the following beneficial effects:

[0036] 1. The present invention optimizes and adjusts the element content of the aluminum alloy raw material, reduces the Fe element content while increasing the Cu element content, and cooperates with the adjusted extrusion process and electrolyte formula to reduce the probability of the profile β-FeSiAl phase, improve the quality of the coloring base color, and can effectively eliminate the two-end color defect that occurs when the aluminum profile is colored dark bronze. The dark bronze base color is ruddy and the coloring quality is good;

[0037] 2. By controlling the temperature of the electrolytic cell, the pH of the electrolyte, and coordinating the homogenization process of the aluminum alloy casting rod, the color uniformity of the upper and lower aluminum profiles is improved;

[0038] 3. The present invention reasonably adjusts the process parameters of each process to ensure that the color of the aluminum profile is uniform and has no obvious defects after the single nickel salt matte deep bronze treatment, thereby improving the surface quality of the aluminum profile. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below in conjunction with specific embodiments.

[0040] The embodiment of the present invention provides a matte dark bronze nickel salt colored aluminum profile and a preparation method thereof.

[0041] Firstly, the raw materials are melted and cast according to the formula to obtain aluminum alloy casting rods, and then homogenized;

[0042] The aluminum profile is composed of the following components by mass percentage: Mg≤0.9%, Si≤0.6%, Fe≤0.2%, Cu≤0.1%, Mn≤0.05%, Ti≤0.05%, Cr≤0.05%, Zn≤0.05%, and the balance is Al;

[0043] Preferably, the aluminum profile is composed of the following components by mass percentage: Mg 0.48-0.53%, Si 0.38-0.41%, Fe ≤ 0.15%, Cu ≤ 0.1%, Mn ≤ 0.05%, Ti ≤ 0.05%, Cr ≤ 0.05%, Zn ≤ 0.05%, and the balance is Al and unavoidable impurities, with a single impurity ≤ 0.05% and a total impurity ≤ 0.15%;

[0044] More preferably, the aluminum profile is composed of the following components by mass percentage: Mg 0.48-0.51%, Si 0.38-0.40%, Fe 0.09-0.15%, Cu 0.08-0.1%, Mn≤0.05%, Ti≤0.05%, Cr≤0.05%, Zn≤0.05%, and the balance is Al and unavoidable impurities, with a single impurity ≤0.05% and a total impurity ≤0.15%;

[0045] In the existing 6063 grade aluminum alloy, there are too many Fe impurity components, resulting in the presence of β-FeSiAl phase in the profile, and the transparency of the oxide film of the aluminum profile is low, and defects such as color turbidity easily occur. The present invention controls the Fe impurity element range to 0.09-0.15%, and correspondingly controls the Cu element range to 0.08-0.1%, which is beneficial to promoting the surface brightness of the aluminum profile, improving the defects of the coloring surface being dark and dull, and having no bronze red background color, and ensuring that the quality of the cast rod meets the demand.

[0046] The aluminum alloy casting rod after homogenization is then extruded to obtain an aluminum profile blank, and then quenched; the upper machine temperature of the aluminum alloy casting rod is lower than the upper machine temperature of the mold;

[0047] Preferably, during the extrusion process, the upper machine temperature of the die is 475-485°C, the outlet temperature of the cast rod is 475-485°C, and the upper machine temperature of the cast rod is 465-475°C; by optimizing the extrusion process, the casting stress is reduced.

[0048] The quenching treatment is a strong wind quenching treatment; if the quenching process does not meet the optimal requirements, the MgSi phase particles in the aluminum alloy structure are unevenly precipitated, and there is a segregation problem on the surface, resulting in the defect that the surface of the aluminum profile is foggy white and the base color is not transparent.

[0049] The electrolytic coloring process of aluminum profiles includes immersing the aluminum profile blank in an electrolyte, performing an electrolytic coloring treatment, and performing a second water washing treatment; the electrolyte is composed of the following components: nickel sulfate with a concentration of 135-150 g / L, boric acid with a concentration of 38-42 g / L, monovalent cations with a concentration of ≤10 ppm, and the balance is water; the monovalent cations include Na + , K + NH4 + , where Na + As the main impurity ion, Na+ The concentration of is controlled within 8ppm. When the total amount of in the tank liquid exceeds 10ppm, special potassium and sodium removal equipment needs to be turned on.

[0050] By optimizing the raw material formula of aluminum alloy and optimizing the extrusion process and electrolyte formula, the probability of two-color appearing on the aluminum profile after coloring can be reduced, which is conducive to obtaining aluminum profiles with good base color and uniform color.

[0051] Furthermore, during the electrolytic coloring process, the pH of the electrolyte is 3.8-4.5, the electrolytic cell temperature is 24-26°C, and the electrolytic coloring time is 225-310s; before electrolytic coloring, the pH range of the single nickel salt coloring tank liquid needs to be measured, and the standard range is 3.8-4.5. If the pH of the tank liquid is less than 3.8, it will cause more acid water to remain in the pores of the oxide film, causing coloring hydrogen reduction, resulting in uneven coloring, and it is necessary to take samples for testing and open the anion exchange tower for adjustment; if the pH of the tank liquid is greater than 4.5, it is necessary to add a small amount of sulfuric acid reagent to adjust the pH.

[0052] The coloring time depends on the required color depth of the aluminum profile. Specifically, sandblasting matte 6# is 70s, sandblasting matte 5# is 118s, sandblasting oxidation 2.5# is 120s, sandblasting matte customization is 160s, and sandblasting matte bronze 8# is 230s.

[0053] The coloring treatment also includes a water washing treatment, and the two water washing times are each 10 seconds.

[0054] Preferably, the temperature of the homogenization treatment is 540°C-560°C, and the time of the homogenization treatment is ≥3.5h;

[0055] After homogenization, the aluminum alloy casting rod is cooled to a rod temperature of 200-210°C by strong wind, and then cooled to room temperature by water mist. If the homogenization time of the casting rod is insufficient, the casting stress will not be completely eliminated, and the segregation of the structure will not be effectively reduced, which will affect the quality of the extruded material and cause the overall base color of the aluminum profile to be uneven.

[0056] Combined with the optimal bath pH, ​​bath temperature and homogenization treatment process, the color uniformity of the aluminum profile can be further improved, avoiding color differences between the upper and lower parts of the aluminum profile.

[0057] In addition, the overall quality of aluminum profiles can be further improved by optimizing other processes.

[0058] (3) sandblasting the aluminum profile;

[0059] The sandblasting process includes a first sandblasting process performed by a first spray gun, and a second sandblasting process performed by a second spray gun;

[0060] The feeding frequency of the first spray gun is 40-50 Hz, the feeding frequency of the second spray gun is 40-50 Hz; the sandblasting recovery frequency of the spray guns is 45-50 Hz.

[0061] The density and thickness of the material sand surface have a key influence on the reflectivity of metal salt deposition after coloring. The greater the sandblasting pressure and the slower the feed speed, the higher the sand surface density and the deeper the sand surface. The higher the height between the sand pit surface and the bottom of the sand pit, the less likely it is to reflect metal salt, resulting in the material being black. Therefore, it is necessary to adjust the feed speed according to the different material cross-sections and reasonably reduce the sandblasting pressure so that the material sand surface can achieve a delicate and bright sand texture.

[0062] The sandblasting process is specifically optimized according to the characteristics of the sand surface, mainly by increasing the sandblasting feed frequency to 45-50Hz, reducing the sand surface density of a single sandblasting, and reducing the density of diffuse reflection, thereby optimizing the problem of black spraying on the sand surface.

[0063] (4) Pretreatment of aluminum profiles after sandblasting;

[0064] Pretreatment includes degreasing, alkali etching and neutralization. Pretreatment is beneficial to cleaning the surface of the profile and ensuring the quality of subsequent coloring.

[0065] The degreasing liquid used in the degreasing treatment has a degreasing component concentration of 60-70 g / L, and the degreasing treatment time is 1-3 min;

[0066] The alkali concentration in the alkali etching solution used in the alkali etching treatment is 90-130g / L, the alkali etching treatment time is 1-3min, and the alkali etching temperature is 45-55°C; after the alkali etching, the trough is entered into the water washing process as soon as possible, the water washing overflow must be strengthened, and industrial new water must be continuously added to prevent the aluminum profiles after the alkali etching from staying in the air;

[0067] The neutralization liquid used in the neutralization treatment is a sulfuric acid solution, the free sulfuric acid concentration in the sulfuric acid solution is 180-200g / L, the neutralization treatment time is 0.5-2min, and two water washes are performed after the neutralization treatment, and the water washing time is 1-20s. After the neutralization treatment, a high-pressure water gun is used to comprehensively clean each hanging material from top to bottom to prevent the material from being drained too quickly and the residual alkali solidified on the surface of the material, resulting in surface flower and other undesirable conditions.

[0068] (5) anodizing the pretreated aluminum profile and performing a first water washing treatment, wherein the first water washing treatment includes three water washing treatments;

[0069] The sulfuric acid concentration in the anodizing solution is 220-280 g / L, the aluminum ion concentration is 10-20 g / L, and the current density during the anodizing process is 120-140 A / m 2, the oxidation tank temperature is 18-20℃, and the oxidation time is 20-30min;

[0070] In the oxidation process, the active surface of oxide film formation is located on the surface of substrate tissue. The grain density of substrate tissue directly affects the growth density and distribution of oxide film. Nickel metal salt is precipitated at the bottom of oxide film, and the difference in color of metal salt in the pores of oxide film is reflected by light refraction. The quality of oxide film formation is affected by key factors such as bath solution concentration, bath temperature, conductivity, current density, and stability of substrate tissue.

[0071] The first water washing treatment includes the first water washing, the second water washing and the third water washing. The pH of the washing liquid in the first water washing is 0.8-1.7, the pH of the washing liquid in the second water washing is 2.1-3.7, and the pH of the washing liquid in the third water washing is 4.0-5.0. The washing time is 20-30s, and the conductivity of the washing liquid is ≤15μS / cm.

[0072] The pH of the single nickel salt bath is lower than that of the single tin salt bath. Therefore, there are strict step-by-step pH regulations for the post-oxidation washing process. If the acidic residual liquid of the material oxidation is not thoroughly cleaned, Na + NH4 + If it is brought into the coloring tank, it will cause contamination of the main tank, causing the impurity ions in the main tank to increase rapidly and the pH to decrease, thus affecting the coloring process.

[0073] (7) The aluminum profile after the second water washing treatment is subjected to matte photophoresis treatment and cured.

[0074] The conductivity of the electrophoresis solution in the electrophoresis main tank is 650-950 μS / cm, the solid content is 9.5-10.5 wt%, the pH is 8.3-8.6, the electrophoresis temperature is 18-22° C., and the electrophoresis voltage is 120-150 V;

[0075] After the matting photophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting photophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing;

[0076] The conductivity of the washing liquid of the RO1 washing tank is ≤250μS / cm, the solid content is 0.3-1.5wt%, and the pH is 8.5-9.5;

[0077] The conductivity of the washing liquid of the RO2 washing tank is ≤125μS / cm, the solid content is 0.1-0.2wt%, and the pH is 8.5-9.5;

[0078] The curing temperature is 180-190℃, and the curing time is 40-50min. Through the curing treatment, the surface of the aluminum profile can achieve certain weather resistance, physical properties and chemical resistance.

[0079] The specific embodiments of the present invention are described in further detail below.

[0080] Embodiment 1: The aluminum profile is composed of the following components by mass percentage: Mg 0.6%, Si 0.5%, Fe 0.2%, Cu 0.1%, Mn 0.05%, Ti 0.05%, Cr 0.05%, Zn 0.05%, and the balance is Al and unavoidable impurities, with a single impurity ≤ 0.05% and a total impurity ≤ 0.15%;

[0081] The preparation process includes the following steps:

[0082] (1) melting and casting the raw materials according to the formula to obtain aluminum alloy cast bars, homogenizing them at 530° C. for 10 h, and cooling them to room temperature with water mist;

[0083] (2) Extruding the homogenized aluminum alloy casting rod to obtain an aluminum profile blank, the upper machine temperature of the mold is 480° C., the upper machine temperature of the aluminum alloy casting rod is 475° C., and the aluminum profile blank is subjected to strong wind quenching treatment;

[0084] (3) sandblasting the aluminum profile blank after quenching, and the feeding frequency of the spray gun is 45 Hz;

[0085] (4) performing pretreatments such as degreasing, alkaline etching and neutralization on the aluminum profile blank after sandblasting;

[0086] (5) The pretreated aluminum profile blank is anodized and subjected to a first water washing treatment. The sulfuric acid concentration of the anodizing treatment solution is 250 g / L, the aluminum ion concentration is 10 g / L, and the current density during the treatment is 125 A / m 2 , the oxidation tank temperature is 20℃, and the oxidation time is 25min;

[0087] The first water washing treatment includes the first water washing, the second water washing and the third water washing. The pH of the washing liquid of the first water washing is 0.8, the pH of the washing liquid of the second water washing is 2.3, and the pH of the washing liquid of the third water washing is 4.0. The washing time of the three water washings is 60s, and the conductivity of the washing liquid is 18μS / cm.

[0088] (6) immersing the aluminum profile blank after the first water washing treatment into an electrolyte for electrolytic coloring treatment, the electrolytic bath temperature is 26° C., the pH is 4.1, the coloring time is 253 s, and a second water washing treatment is performed;

[0089] The electrolyte includes the following components: nickel sulfate at a concentration of 145 g / L, boric acid at a concentration of 42 g / L, and monovalent cations at a concentration of ≤10 ppm;

[0090] (7) The aluminum profile blank after the second water washing treatment is subjected to matting electrophoresis treatment, the electrophoresis solution in the electrophoresis main tank has a pH of 8.5, a conductivity of 800 μS / cm, a solid content of 10 wt %, an electrophoresis temperature of 20° C., and an electrophoresis voltage of 120 V;

[0091] After the electrophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting electrophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing; the water washing liquid of the RO1 washing tank has a conductivity of 250 μS / cm, a solid content of 0.8wt%, and a pH of 9.0; the water washing liquid of the RO2 washing tank has a conductivity of 125 μS / cm, a solid content of 0.1wt%, and a pH of 8.5;

[0092] The aluminum profile blank after the third water washing treatment is cured at a curing temperature of 185° C. for 45 minutes to obtain a finished product.

[0093] Embodiment 2: The aluminum profile is composed of the following components by mass percentage: Mg 0.5%, Si 0.41%, Fe 0.15%, Cu 0.1%, Mn 0.02%, Ti 0.02%, Cr 0.02%, Zn 0.02%, and the balance is Al and unavoidable impurities, with a single impurity ≤ 0.05% and a total impurity ≤ 0.15%;

[0094] The preparation process includes the following steps:

[0095] (1) The raw materials are melted and cast according to the formula to obtain aluminum alloy cast bars, which are homogenized at 570° C. for 11 h and then cooled to room temperature by water mist;

[0096] (2) Extruding the homogenized aluminum alloy casting rod to obtain an aluminum profile blank, the upper machine temperature of the mold is 475° C., the upper machine temperature of the aluminum alloy casting rod is 470° C., and the aluminum profile blank is subjected to strong wind quenching treatment;

[0097] (3) sandblasting the aluminum profile blank after quenching, and the feeding frequency of the spray gun is 50 Hz;

[0098] (4) performing pretreatments such as degreasing, alkaline etching and neutralization on the aluminum profile blank after sandblasting;

[0099] (5) The pretreated aluminum profile blank is anodized and subjected to a first water washing treatment. The sulfuric acid concentration of the anodizing treatment solution is 270 g / L, the aluminum ion concentration is 15 g / L, and the current density during the treatment is 140 A / m 2 , the oxidation tank temperature is 20℃, and the oxidation time is 25min;

[0100] The first water washing treatment includes the first water washing, the second water washing and the third water washing. The pH of the washing liquid of the first water washing is 1.7, the pH of the washing liquid of the second water washing is 2.1, and the pH of the washing liquid of the third water washing is 4.4. The washing time of the three water washings is 30 seconds, and the conductivity of the washing liquid is 12μS / cm.

[0101] (6) immersing the aluminum profile blank after the first water washing treatment into an electrolyte for electrolytic coloring treatment, wherein the electrolytic bath temperature is 24° C., the pH is 4.3, the coloring time is 230 s, and a second water washing treatment is performed;

[0102] The electrolyte includes the following components: nickel sulfate at a concentration of 150 g / L, boric acid at a concentration of 42 g / L, and monovalent cations at a concentration of 8 ppm;

[0103] (7) The aluminum profile blank after the second water washing treatment is subjected to matting electrophoresis treatment, the electrophoresis solution in the electrophoresis main tank has a pH of 8.5, a conductivity of 750 μS / cm, a solid content of 10 wt %, an electrophoresis temperature of 20° C., and an electrophoresis voltage of 140 V;

[0104] After the electrophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting electrophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing; the water washing liquid of the RO1 washing tank has a conductivity of 250 μS / cm, a solid content of 0.8wt%, and a pH of 9.0; the water washing liquid of the RO2 washing tank has a conductivity of 150 μS / cm, a solid content of 0.1wt%, and a pH of 8.5;

[0105] The aluminum profile blank after the third water washing treatment is cured at a curing temperature of 185° C. for 45 minutes to obtain a finished product.

[0106] Embodiment 3: The aluminum profile is composed of the following components by mass percentage: Mg 0.48%, Si 0.38%, Fe 0.09%, Cu 0.08%, Mn 0.02%, Ti 0.02%, Cr 0.02%, Zn 0.02%, and the balance is Al and unavoidable impurities, with a single impurity ≤ 0.05% and a total impurity ≤ 0.15%;

[0107] The preparation process includes the following steps:

[0108] (1) The raw materials are melted and cast according to the formula to obtain aluminum alloy cast bars, which are homogenized at 560° C. for 12 h and then cooled to room temperature by water mist;

[0109] (2) Extruding the homogenized aluminum alloy casting rod to obtain an aluminum profile blank, the upper machine temperature of the mold is 480° C., the upper machine temperature of the aluminum alloy casting rod is 470° C., and the aluminum profile blank is subjected to strong wind quenching treatment;

[0110] (3) sandblasting the aluminum profile blank after quenching, and the feeding frequency of the spray gun is 50 Hz;

[0111] (4) performing pretreatments such as degreasing, alkaline etching and neutralization on the aluminum profile blank after sandblasting;

[0112] (5) The pretreated aluminum profile blank is anodized and subjected to a first water washing treatment. The sulfuric acid concentration of the anodizing treatment solution is 260 g / L, the aluminum ion concentration is 10 g / L, and the current density during the treatment is 130 A / m 2 , the oxidation tank temperature is 20℃, and the oxidation time is 25min;

[0113] The first water washing treatment includes the first water washing, the second water washing and the third water washing. The pH of the washing liquid of the first water washing is 1.5, the pH of the washing liquid of the second water washing is 2.5, and the pH of the washing liquid of the third water washing is 4.5. The washing time of the three water washings is 60s, and the conductivity of the washing liquid is 10μS / cm.

[0114] (6) immersing the aluminum profile blank after the first water washing treatment into an electrolyte for electrolytic coloring treatment, wherein the electrolytic bath temperature is 25° C., the pH is 4.0, the coloring time is 230 s, and a second water washing treatment is performed;

[0115] The electrolyte includes the following components: nickel sulfate at a concentration of 150 g / L, boric acid at a concentration of 42 g / L, and monovalent cations at a concentration of 8 ppm;

[0116] (7) subjecting the aluminum profile blank after the second water washing treatment to matting electrophoresis treatment, wherein the electrophoresis solution in the electrophoresis main tank has a pH of 8.5, a conductivity of 800 μS / cm, a solid content of 10 wt %, an electrophoresis temperature of 20° C., and an electrophoresis voltage of 140 V;

[0117] After the electrophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting electrophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing; the water washing liquid of the RO1 washing tank has a conductivity of 200 μS / cm, a solid content of 0.8wt%, and a pH of 9.0; the water washing liquid of the RO2 washing tank has a conductivity of 100 μS / cm, a solid content of 0.1wt%, and a pH of 8.5;

[0118] The aluminum profile blank after the third water washing treatment is cured at a curing temperature of 185° C. for 45 minutes to obtain a finished product.

[0119] Comparative Example 1: The aluminum profile is composed of the following components by mass percentage: Mg 0.6%, Si 0.5%, Fe 0.2%, Cu 0.1%, Mn 0.05%, Ti 0.05%, Cr 0.05%, Zn 0.05%, and the balance is Al and unavoidable impurities, with a single impurity ≤0.05% and a total impurity ≤0.15%;

[0120] The preparation process includes the following steps:

[0121] (1) melting and casting the raw materials according to the formula to obtain aluminum alloy cast bars, homogenizing them at 530° C. for 10 h, and cooling them to room temperature with water mist;

[0122] (2) Extruding the homogenized aluminum alloy casting rod to obtain an aluminum profile blank, the upper machine temperature of the mold is 465° C., the upper machine temperature of the aluminum alloy casting rod is 500° C., and the aluminum profile blank is subjected to strong wind quenching treatment;

[0123] (3) sandblasting the aluminum profile blank after quenching, and the feeding frequency of the spray gun is 45 Hz;

[0124] (4) performing pretreatments such as degreasing, alkaline etching and neutralization on the aluminum profile blank after sandblasting;

[0125] (5) The pretreated aluminum profile blank is anodized and subjected to a first water washing treatment. The sulfuric acid concentration of the anodizing treatment solution is 250 g / L, the aluminum ion concentration is 10 g / L, and the current density during the treatment is 125 A / m 2 , the oxidation tank temperature is 20℃, and the oxidation time is 25min;

[0126] The first water washing treatment includes the first water washing, the second water washing and the third water washing. The pH of the washing liquid of the first water washing is 0.8, the pH of the washing liquid of the second water washing is 2.3, and the pH of the washing liquid of the third water washing is 4.0. The washing time of the three water washings is 25 seconds, and the conductivity of the washing liquid is 12μS / cm.

[0127] (6) immersing the aluminum profile blank after the first water washing treatment in an electrolyte for electrolytic coloring treatment, wherein the electrolytic bath temperature is 26° C., the pH is 3.5, the coloring time is 230 s, and a second water washing treatment is performed;

[0128] The electrolyte includes the following components: nickel sulfate at a concentration of 130 g / L, boric acid at a concentration of 35 g / L, and monovalent cations at a concentration of 12 ppm;

[0129] (7) The aluminum profile blank after the second water washing treatment is subjected to matting electrophoresis treatment, the electrophoresis solution in the electrophoresis main tank has a pH of 8.5, a conductivity of 800 μS / cm, a solid content of 10 wt %, an electrophoresis temperature of 18° C., and an electrophoresis voltage of 120 V;

[0130] After the electrophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting electrophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing; the water washing liquid of the RO1 washing tank has a conductivity of 200 μS / cm, a solid content of 0.8wt%, and a pH of 9.0; the water washing liquid of the RO2 washing tank has a conductivity of 100 μS / cm, a solid content of 0.1wt%, and a pH of 8.5;

[0131] The aluminum profile blank after the third water washing treatment is cured at a curing temperature of 185° C. for 45 minutes to obtain a finished product.

[0132] Comparative Example 2: The aluminum profile is composed of the following components by mass percentage: Mg 0.6%, Si 0.5%, Fe 0.35%, Cu 0.04%, Mn 0.05%, Ti 0.05%, Cr 0.05%, Zn 0.05%, and the balance is Al and unavoidable impurities, with a single impurity ≤ 0.05% and a total impurity ≤ 0.15%;

[0133] The preparation process includes the following steps:

[0134] (1) The raw materials are melted and cast according to the formula to obtain aluminum alloy cast bars, which are homogenized at 530° C. for 3 h and then cooled to room temperature by water mist;

[0135] (2) Extruding the homogenized aluminum alloy casting rod to obtain an aluminum profile blank, the upper machine temperature of the mold is 475° C., the upper machine temperature of the aluminum alloy casting rod is 475° C., and the aluminum profile blank is subjected to strong wind quenching treatment;

[0136] (3) sandblasting the aluminum profile blank after quenching, and the feeding frequency of the spray gun is 45 Hz;

[0137] (4) performing pretreatments such as degreasing, alkaline etching and neutralization on the aluminum profile blank after sandblasting;

[0138] (5) The pretreated aluminum profile blank is anodized and subjected to a first water washing treatment. The sulfuric acid concentration of the anodizing treatment solution is 250 g / L, the aluminum ion concentration is 10 g / L, and the current density during the treatment is 125 A / m 2 , the oxidation tank temperature is 20℃, and the oxidation time is 25min;

[0139] The first water washing treatment includes the first water washing, the second water washing and the third water washing. The pH of the washing liquid of the first water washing is 0.8, the pH of the washing liquid of the second water washing is 2.3, and the pH of the washing liquid of the third water washing is 4.0. The washing time of the three water washings is 25 seconds, and the conductivity of the washing liquid is 12μS / cm.

[0140] (6) immersing the aluminum profile blank after the first water washing treatment in an electrolyte for electrolytic coloring treatment, wherein the electrolytic bath temperature is 26° C., the pH is 3.5, the coloring time is 230 s, and a second water washing treatment is performed;

[0141] The electrolyte includes the following components: nickel sulfate at a concentration of 130 g / L, boric acid at a concentration of 35 g / L, and monovalent cations at a concentration of 12 ppm;

[0142] (7) The aluminum profile blank after the second water washing treatment is subjected to matting electrophoresis treatment, the electrophoresis solution in the electrophoresis main tank has a pH of 8.5, a conductivity of 800 μS / cm, a solid content of 10 wt %, an electrophoresis temperature of 18° C., and an electrophoresis voltage of 120 V;

[0143] After the electrophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting electrophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing; the water washing liquid of the RO1 washing tank has a conductivity of 200 μS / cm, a solid content of 0.8wt%, and a pH of 9.0; the water washing liquid of the RO2 washing tank has a conductivity of 100 μS / cm, a solid content of 0.1wt%, and a pH of 8.5;

[0144] The aluminum profile blank after the third water washing treatment is cured at a curing temperature of 185° C. for 45 minutes to obtain a finished product.

[0145] Comparative Example 3: The aluminum profile is composed of the following components by mass percentage: Mg 0.6%, Si 0.5%, Fe 0.35%, Cu 0.04%, Mn 0.05%, Ti 0.05%, Cr 0.05%, Zn 0.05%, and the balance is Al and unavoidable impurities, with a single impurity ≤ 0.05% and a total impurity ≤ 0.15%;

[0146] The preparation process includes the following steps:

[0147] (1) The raw materials are melted and cast according to the formula to obtain aluminum alloy cast bars, which are homogenized at 530° C. for 3 h and then cooled to room temperature by water mist;

[0148] (2) Extruding the homogenized aluminum alloy casting rod to obtain an aluminum profile blank, the upper machine temperature of the mold is 465° C., the upper machine temperature of the aluminum alloy casting rod is 500° C., and the aluminum profile blank is subjected to strong wind quenching treatment;

[0149] (3) sandblasting the aluminum profile blank after quenching, and the feeding frequency of the spray gun is 45 Hz;

[0150] (4) performing pretreatments such as degreasing, alkaline etching and neutralization on the aluminum profile blank after sandblasting;

[0151] (5) The pretreated aluminum profile blank is anodized and subjected to a first water washing treatment. The sulfuric acid concentration of the anodizing treatment solution is 250 g / L, the aluminum ion concentration is 10 g / L, and the current density during the treatment is 125 A / m 2 , the oxidation tank temperature is 20℃, and the oxidation time is 25min;

[0152] The first water washing treatment includes the first water washing, the second water washing and the third water washing. The pH of the washing liquid of the first water washing is 0.8, the pH of the washing liquid of the second water washing is 2.3, and the pH of the washing liquid of the third water washing is 4.0. The washing time of the three water washings is 25 seconds, and the conductivity of the washing liquid is 12μS / cm.

[0153] (6) immersing the aluminum profile blank after the first water washing treatment in an electrolyte for electrolytic coloring treatment, wherein the electrolytic bath temperature is 26° C., the pH is 3.5, the coloring time is 230 s, and a second water washing treatment is performed;

[0154] The electrolyte includes the following components: nickel sulfate at a concentration of 135 g / L, boric acid at a concentration of 38 g / L, and monovalent cations at a concentration of 10 ppm;

[0155] (7) The aluminum profile blank after the second water washing treatment is subjected to matting electrophoresis treatment, the electrophoresis solution in the electrophoresis main tank has a pH of 8.5, a conductivity of 800 μS / cm, a solid content of 10 wt %, an electrophoresis temperature of 18° C., and an electrophoresis voltage of 120 V;

[0156] After the electrophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting electrophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing; the water washing liquid of the RO1 washing tank has a conductivity of 200 μS / cm, a solid content of 0.8wt%, and a pH of 9.0; the water washing liquid of the RO2 washing tank has a conductivity of 100 μS / cm, a solid content of 0.1wt%, and a pH of 8.5;

[0157] The aluminum profile blank after the third water washing treatment is cured at a curing temperature of 185° C. for 45 minutes to obtain a finished product.

[0158] Performance testing:

[0159] According to GB / T 12967.6-2022, the aluminum profiles prepared in Examples 1-3 and Comparative Examples 1-3 were tested for color difference and appearance quality. The height of the aluminum profiles was 6m.

[0160] 1. CIE chromaticity: measured at 3m in height direction of aluminum profile;

[0161] 2. Color difference between the two ends: measure at 0.2m from the upper and lower ends of the aluminum profile, and calculate △E1 according to the following formula;

[0162]

[0163] Where, L1 * 、a1 * and b1 * They are the brightness, red-green index and yellow-blue index at 0.2m from the top of the aluminum profile, L2 * 、a2 * and b2 * They are the brightness, red-green index and yellow-blue index at 0.2m from the lower end of the aluminum profile;

[0164] 3. Color difference between upper and lower parts: Measure at 0.5m, 1.5m and 2.5m from the upper and lower ends of the aluminum profile, and calculate △E according to the following formula: 2i , and calculate the average value of several as the upper and lower color difference △E2;

[0165]

[0166] Where, L 1i * 、a 1i * and b 1i * are the brightness, red-green index and yellow-blue index at the i-th point from the upper end of the aluminum profile (i is 0.5m, 1.5m and 2.5m respectively), L 2i * 、a 2i * and b 2i * They are the brightness, red-green index and yellow-blue index at the i-th point (i is 0.5m, 1.5m and 2.5m) from the lower end of the aluminum profile;

[0167] 4. Defects: Use visual inspection to observe whether the sample has defects. If there is no white fog, wrinkles, cracks, bubbles, flow marks, pockmarks, inclusions, stickiness or paint film falling off on the surface of the sample, it is considered to be free of defects.

[0168] The test results are shown in Table 1.

[0169] Table 1 Aluminum profile performance test

[0170]

[0171] From the comparison between comparative examples 1-3 and embodiment 1, it can be seen that only by simultaneously adopting the preferred aluminum profile raw material formula, extrusion process and electrolyte formula, can a uniformly colored aluminum profile be obtained. If only one of the process formulas is preferred, the obtained aluminum profile is dark and matte and the color is uneven, especially the color at both ends is more serious. The color at both ends of the aluminum profile in embodiment 1 is significantly alleviated. From the comparison between embodiment 3 and embodiments 1 and 2, it can be seen that by optimizing the pH and tank temperature of the coloring tank liquid and performing preferred homogenization treatment, the probability of upper and lower color differences in the aluminum profile can be further reduced. The aluminum profile produced by the present invention has no defects such as surface flowers, has uniform color, a deep bronze base color, a good rosy gloss, and a good surface quality, which can meet the use requirements.

[0172] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing a matte dark bronze nickel salt colored aluminum profile, characterized in that: The following steps are involved: (1) melting and casting the raw materials according to the formula to obtain aluminum alloy cast rods, and homogenizing the raw materials, wherein the raw materials are composed of the following components by mass percentage: Mg≤0.9%, Si≤0.6%, Fe≤0.2%, Cu≤0.1%, Mn≤0.05%, Ti≤0.05%, Cr≤0.05%, Zn≤0.05%, and the balance is Al and unavoidable impurities, with a single impurity of ≤0.05% and a total impurity of ≤0.15%; (2) Extruding the homogenized aluminum alloy casting rod to obtain an aluminum profile blank, and quenching the blank; the upper machine temperature of the aluminum alloy casting rod after the homogenization treatment is lower than the upper machine temperature of the mold, the upper machine temperature of the aluminum alloy casting rod is 465-475° C., and the upper machine temperature of the mold is 475-485° C.; (3) sandblasting the aluminum profile blank after quenching; (4) pre-treating the aluminum profile blank after sandblasting; (5) subjecting the pretreated aluminum profile blank to anodizing treatment and performing a first water washing treatment; The pretreated aluminum profile blank is immersed in an anodizing treatment solution and energized. The sulfuric acid concentration in the anodizing treatment solution is 220-280 g / L, the aluminum ion concentration is 10-20 g / L, and the current density during the anodizing treatment is 120-140 A / m 2 , the oxidation tank temperature is 18-20℃, and the oxidation time is 20-30min; The first water washing treatment includes a first water washing treatment, a second water washing treatment and a third water washing treatment; The pH of the washing liquid in the first washing treatment is 0.8-1.7, the washing time is 20-30s, and the conductivity of the washing liquid is ≤15μS / cm; The pH of the washing liquid in the second washing treatment is 2.1-3.7, the washing time is 20-30s, and the conductivity of the washing liquid is ≤15μS / cm; The pH of the washing liquid in the third washing treatment is 4.0-5.0, the washing time is 20-30s, and the conductivity of the washing liquid is ≤15μS / cm; (6) immersing the aluminum profile blank after the first water washing treatment into an electrolyte, performing an electrolytic coloring treatment, and performing a second water washing treatment; The pH of the electrolyte is 3.8-4.5, the temperature of the electrolytic cell is 24-26°C, and the electrolytic coloring time is 225-310s; The electrolyte comprises the following components: nickel sulfate at a concentration of 135-150 g / L, boric acid at a concentration of 38-42 g / L, and monovalent cations at a concentration of ≤10 ppm; The second washing time is 1-10s; (7) subjecting the aluminum profile blank after the second water washing treatment to matting photophoresis treatment and curing; The aluminum profile blank after the second water washing treatment is immersed in an electrophoresis solution for extinction electrophoresis treatment, wherein the electrophoresis solution has a pH of 8.3-8.6, a conductivity of 650-950 μS / cm, a solid content of 9.5-10.5 wt %, an electrophoresis temperature of 18-22° C., and an electrophoresis voltage of 120-150 V; After the matting photophoresis treatment, a third water washing treatment is performed, and the third water washing treatment includes putting the aluminum profile blank after the matting photophoresis treatment into the RO1 washing tank and the RO2 washing tank for washing; The conductivity of the washing liquid of the RO1 washing tank is ≤250μS / cm, the solid content is 0.3-1.5wt%, and the pH is 8.5-9.5; The conductivity of the washing liquid of the RO2 washing tank is ≤125μS / cm, the solid content is 0.1-0.2wt%, and the pH is 8.5-9.5; The aluminum profile blank after the third water washing treatment is cured at a temperature of 180-190° C. and a curing time of 40-50 minutes.

2. The method for preparing the matte dark bronze nickel salt colored aluminum profile according to claim 1, characterized in that: The aluminum profile is composed of the following components by mass percentage: Mg 0.48-0.53%, Si 0.38-0.41%, Fe0.01-0.15%, Cu 0.01-0.1%, Mn 0.01-0.05%, Ti 0.01-0.05%, Cr 0.01-0.05%, Zn0.01-0.05%, the balance is Al and unavoidable impurities, the impurities are 0.01-0.05% individually and 0.01-0.15% in total.

3. The method for preparing the matte dark bronze nickel salt colored aluminum profile according to claim 1, characterized in that: In step (2), the quenching treatment is a strong wind quenching treatment.

4. The method for preparing the matte dark bronze nickel salt colored aluminum profile according to claim 1, characterized in that: In step (1), the temperature of the homogenization treatment is 540°C-560°C, and the time of the homogenization treatment is ≥10h; after the homogenization treatment is completed, the aluminum alloy casting rod is cooled by strong wind for 4-6h until the rod temperature is 200-210°C, and then cooled to room temperature by water mist.

5. The method for preparing the matte dark bronze nickel salt colored aluminum profile according to claim 1, characterized in that: In step (4), the pretreatment includes degreasing treatment, alkaline etching treatment and neutralization treatment in sequence; The degreasing liquid used in the degreasing treatment has a degreasing component concentration of 60-70 g / L, and the degreasing treatment time is 1-3 min; The alkali concentration in the alkali etching solution used in the alkali etching treatment is 90-130 g / L, the alkali etching treatment time is 1-3 min, and the alkali etching temperature is 45-55° C. The neutralization liquid used in the neutralization treatment is a sulfuric acid solution, the concentration of free sulfuric acid in the sulfuric acid solution is 180-200 g / L, and the neutralization treatment time is 0.5-2 min.