A method for preparing electrolytic manganese slag brick

By ball milling and calcining electrolytic manganese slag with magnesium oxide and calcium oxide, and combining the proportions of clay, ceramsite and cement for three-stage firing, the problem of solidification and low absorption of manganese ions in the treatment of electrolytic manganese slag is solved. Efficient manganese slag brick preparation is achieved, reducing environmental pollution and health risks.

CN116835963BActive Publication Date: 2024-10-18HUNAN ACAD OF ENVIRONMENTAL PROTECTION SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310818513.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-05
Publication Date
2024-10-18
Estimated Expiration
2043-07-05

AI Technical Summary

Technical Problem

The existing electrolytic manganese slag treatment method has problems with land occupation and harmful substances escaping or escaping. Moreover, its absorption capacity in cement retarder and roadbed materials is low, and it is unable to effectively control the solidification of manganese, resulting in environmental and health risks.

Method used

By ball milling electrolytic manganese slag with magnesium oxide, calcium oxide and water and then calcining, combined with the proportion of clay, ceramsite and cement, a three-stage firing is performed to achieve solidification of manganese ions and high-strength preparation of bricks, reducing manganese of dissociation and escape.

Benefits of technology

It increases the absorption capacity of electrolytic manganese slag and the compressive strength of bricks, reduces the dissociation and escape of manganese ions, reduces pollution to the environment and soil, and achieves harmless treatment of electrolytic manganese slag and efficient utilization of resources. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116835963B_ABST
    Figure CN116835963B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of converting solid waste into useful or harmless materials, and discloses a method for preparing electrolytic manganese slag bricks. The method comprises the following steps: ball-milling electrolytic manganese slag with magnesium oxide, calcium oxide and water to obtain a preliminary mixture, and then calcining the mixture to obtain material A for standby use; grinding material A, filtering out powder below 150 mesh for standby use; mixing electrolytic manganese slag powder, clay, ceramsite, cement and water in a weight ratio of 5:1:1:1:1:1-2, and mixing them evenly to form a green embryo; finally preheating the green embryo and then firing the green embryo to obtain electrolytic manganese slag bricks. The present invention can improve the absorption capacity of electrolytic manganese slag, and can also realize the solidification of free manganese ions in electrolytic manganese slag, and reduce the adverse effects of manganese escape on soil, environment or human body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of converting solid waste into useful or harmless materials, and in particular relates to a method for preparing electrolytic manganese slag bricks. Background Art

[0002] my country is the world's largest producer, consumer and exporter of electrolytic manganese, accounting for about 98% of the world's total manganese output. In the process of electrolytic manganese, after the manganese ore powder is leached with sulfuric acid, the solid-liquid separation of the slurry will produce wet leaching slag with a water content of about 28%, namely electrolytic manganese slag.

[0003] There are two main methods for treating electrolytic manganese slag: landfill and solidification. The landfill method is to directly landfill the electrolytic manganese slag, which will cause a large area of ​​land resources to be occupied. Moreover, the electrolytic manganese slag contains a large amount of harmful substances such as ammonia nitrogen and soluble manganese ions. During landfill, the harmful substances will become free or escape, causing harm to the surrounding soil ecosystem and even damaging the health of surrounding residents.

[0004] The solidification principle is to transform electrolytic manganese slag into a non-flowing dense solid, including use as cement retarder, production of sulphoaluminate cement, production of crop fertilizer, use as roadbed material (made into electrolytic manganese slag bricks), etc. When used as cement retarder and production of sulphoaluminate cement, due to the inherent characteristics of electrolytic manganese slag, its retarding performance and product strength are not as good as cement produced by adding natural gypsum; and the amount of electrolytic manganese slag added is small, and the absorption capacity is low. When producing crop fertilizer, the heavy metals in electrolytic manganese slag will be deposited in the soil, and long-term use will damage the soil. There are two ways to use it as roadbed material. One is to reduce the ratio of electrolytic manganese slag, which can effectively control the leached manganese content, but its absorption capacity is low, only about 40%; the other is to increase the ratio of electrolytic manganese slag, which can effectively increase the absorption capacity, but it cannot control the solidification of manganese, and manganese will escape and become free during use.

[0005] Therefore, how to increase the consumption capacity and achieve harmless treatment of electrolytic manganese slag is an urgent problem to be solved in the electrolytic manganese industry. Summary of the invention

[0006] The present invention is intended to provide a method for preparing electrolytic manganese slag bricks, and the present invention aims to solve the technical problems existing in the prior art.

[0007] To achieve the above object, the present invention provides the following technical solution, a method for preparing electrolytic manganese slag brick, comprising the following steps:

[0008] Step 1: ball-milling electrolytic manganese slag with magnesium oxide, calcium oxide and water to obtain a preliminary mixture, and then calcining to obtain material A for standby use;

[0009] Step 2: Grind material A, and then filter out the powder below 150 mesh for later use;

[0010] Step 3: mixing electrolytic manganese slag powder, clay, ceramsite, cement and water in a weight ratio of 5:1:1:1:1-2, and evenly mixing to form a green embryo;

[0011] Step 4: preheat the green embryo and then fire it to obtain electrolytic manganese slag bricks.

[0012] Beneficial effects of this technical solution:

[0013] By ball milling the electrolytic manganese slag with magnesium oxide and calcium oxide, the electrolytic manganese slag can be fully contacted and mixed with magnesium oxide and calcium oxide, and the free manganese ions in the electrolytic manganese slag can be solidified during the calcination process, thereby reducing the free or escaped manganese in subsequent use.

[0014] By pre-treating the electrolytic manganese slag, the free manganese ions can be solidified, and then electrolytic manganese slag bricks can be made by proportioning electrolytic manganese slag powder, clay, expanded clay, cement and water. This can ensure that the strength of the bricks is high and the consumption of the electrolytic manganese slag is increased.

[0015] In another preferred embodiment of the present invention, in step 1, the weight ratio of electrolytic manganese slag, magnesium oxide, calcium oxide and water is 7-9:1:1.5:5.

[0016] In another preferred embodiment of the present invention, in step 1, pyrite is added during ball milling, and the weight ratio of pyrite to electrolytic manganese slag is 1:14-18.

[0017] Beneficial effect: Adding pyrite can replace more manganese ions during ball milling and complete the solidification of manganese ions, avoiding the free or escape of manganese ions during the subsequent use of bricks, which will affect the external environment and soil.

[0018] In another preferred embodiment of the present invention, in step 1, the calcination temperature is 700-900° C., and the calcination time is 30-90 min.

[0019] In another preferred embodiment of the present invention, step three further comprises lime, and the weight ratio of lime to electrolytic manganese slag powder is 1:15.

[0020] Beneficial effect: When preparing green embryos, adding lime will not have a significant impact on the absorption capacity of electrolytic manganese slag, and at the same time can achieve the solidification of free manganese ions again.

[0021] In another preferred embodiment of the present invention, in step 4, during preheating, the temperature is increased at a rate of 5°C / min until the temperature reaches 250-400°C, and preheated at this temperature for 30-50 minutes.

[0022] In another preferred embodiment of the present invention, in step 4, during firing, the temperature is increased at a rate of 15°C / min until the temperature reaches 800-1300°C, and fired at this temperature for 1.5-3h.

[0023] In another preferred embodiment of the present invention, in step four, three-stage firing is performed.

[0024] In another preferred embodiment of the present invention, in step four, the firing temperature of the first stage is 800-950°C, and the firing time is 20-40 min; the firing temperature of the second stage is 950-1100°C, and the firing time is 40-80 min; the firing temperature of the third stage is 1100-1300°C, and the firing time is 30-60 min.

[0025] In summary, the beneficial effects of the present invention are:

[0026] 1. The present invention realizes the resource integration and reuse of electrolytic manganese slag. The use of electrolytic manganese slag to prepare bricks can reduce the use of non-renewable resources such as commonly used raw materials such as clay, pottery sand, and crushed stone, and realizes the treatment of electrolytic manganese slag.

[0027] 2. When the electrolytic manganese slag is used as a raw material for preparing bricks, the present invention can process the ammonia nitrogen substances and manganese ions contained in the electrolytic manganese slag to avoid the escape of harmful substances and the adverse effects on the environment, soil and human body.

[0028] 3. The present invention pre-treats the electrolytic manganese slag, and can realize hydration reaction between ammonia nitrogen substances, calcium oxide and water during ball milling to generate ammonia gas and discharge it, thereby treating the ammonia nitrogen substances in the electrolytic manganese slag; at the same time, pyrite is added during ball milling to displace the manganese ions in the electrolytic manganese slag, and then combined with calcination after ball milling, the manganese ions react with magnesium oxide and calcium oxide to complete the solidification of the manganese ions, thereby avoiding the free and escape of manganese ions after the subsequent brick making, thereby avoiding adverse effects on the external environment, soil and human body.

[0029] 4. The manganese in the electrolytic manganese slag mainly exists in the form of divalent manganese and tetravalent manganese. During the stacking process, the particles gradually form hard blocks, and the soluble divalent manganese will gradually be oxidized to tetravalent manganese, which is not easy to leach, but also not easy to solidify. Therefore, when using electrolytic manganese slag as a raw material to prepare bricks, manganese will be free and escape in subsequent use. The present invention can reduce the occurrence of manganese free and escape in subsequent use by replacing tetravalent manganese ions and completing solidification.

[0030] 5. The present invention can improve the stability of the electrolytic manganese slag and thus improve the compressive strength of the prepared bricks by calcining the electrolytic manganese slag before making bricks. When the proportion of the electrolytic manganese slag is relatively high, the compressive strength of the bricks can reach the standard, thereby increasing the consumption of the electrolytic manganese slag.

[0031] 6. The present invention uses a three-stage firing method. By gradually increasing the firing temperature, it can promote the development and growth of the internal crystal structure of the brick, thereby improving the mechanical properties of the brick body; at the same time, it can also avoid the "overburning" phenomenon.

[0032] In summary, since electrolytic manganese slag contains harmful substances, the present invention can solidify the harmful substances by pre-treating the electrolytic manganese slag, and improve the stability of the electrolytic manganese slag itself, providing a good foundation for subsequent brick making, so that bricks can be made under high-ratio electrolytic manganese slag. It can increase the absorption capacity and reduce the impact of harmful substances escaping on the external environment.

[0033] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0035] Figure 1 It is a step diagram of an embodiment of the present application.

[0036] Figure 2 It is a schematic diagram of the electrolytic manganese slag brick prepared in the embodiment of the present application. DETAILED DESCRIPTION

[0037] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0038] The present invention provides a method for preparing electrolytic manganese slag bricks, such as Figure 1 As shown, the following steps are included:

[0039] Step 1: Pretreatment of electrolytic manganese slag

[0040] Electrolytic manganese slag, magnesium oxide, calcium oxide and water are prepared in a weight ratio of 7 to 9:1:1.5:5 and put into a ball mill for ball milling. During the ball milling process, pyrite is also added, and the weight ratio of pyrite to electrolytic manganese slag is 1:14 to 18. The ball milling speed is 200 to 300 rpm / min, and the ball milling time is 35 to 45 minutes. Then stand for 20 to 30 minutes.

[0041] In this process, manganese ions can be replaced by ball milling and combined with pyrite, which is convenient for the subsequent manganese ion solidification reaction. At the same time, calcium oxide reacts with ammonia nitrogen substances under ball milling conditions to form ammonia gas, which can be discharged and collected when standing.

[0042] The preliminary mixture obtained after ball milling is then calcined to obtain material A for standby use. The calcination temperature is 700-900° C. and the calcination time is 30-90 min.

[0043] During calcination, manganese ions react with magnesium oxide and calcium oxide to complete the solidification of manganese ions and improve the strength characteristics of the electrolytic manganese slag itself.

[0044] Step 2: Grinding of material A

[0045] The material A obtained in step 1 is ground and then filtered to filter out powder below 150 mesh for later use.

[0046] Step 3: Prepare embryos

[0047] Electrolytic manganese slag powder, clay, ceramsite, cement, lime and water are mixed in a weight ratio of 15:3:3:3:1:3-6, and then made into a raw embryo for later use.

[0048] Step 4: Firing

[0049] First, the green embryo prepared in step 3 is preheated at a rate of 5°C / min until the temperature reaches 250-400°C, and then preheated at this temperature for 30-50 minutes.

[0050] Then, the firing is carried out in three stages. In the first firing stage, the temperature is raised at a rate of 15°C / min until the temperature reaches 800-950°C, and then the firing is carried out for 20-40 minutes. In the second firing stage, the firing temperature reaches 950-1100°C and then the firing is carried out for 40-80 minutes. In the third firing stage, the firing temperature reaches 1100-1300°C and then the firing is carried out for 30-60 minutes. Figure 2 The electrolytic manganese slag brick shown.

[0051] By gradually increasing the firing temperature, the development and growth of the internal crystal of the topic can be promoted, which is beneficial to improving the mechanical properties of the brick body; at the same time, it can also avoid the phenomenon of "overburning".

[0052] experiment:

[0053] Electrolytic manganese slag bricks were made according to the preparation method and various parameters provided by the present invention, and the compressive strength, water absorption rate, bulk density and toxic leaching data of the bricks were tested.

[0054] The compressive strength test method is: use a compressive strength test machine to complete the compressive strength test of the brick body, and the compressive machine is set at a speed of 0.6kN / s.

[0055] The test method for water absorption is: dry the brick to be tested at 100°C and keep its weight constant, and measure its weight as m0. Then soak the dried brick in water for 24 hours, measure its weight as m1. Then substitute the weights obtained twice into the following formula to calculate the water absorption of the brick to be tested.

[0056]

[0057] The test method of volume density is: dry the brick to be tested at 100°C to a constant weight, measure its weight and mark it as m0, and then use the Archimedean method to measure its volume, marked as V. Substitute the measured weight m0 and volume V into the following formula to calculate the volume density of the brick to be tested.

[0058]

[0059] The testing method for toxic leaching data is: the manufactured bricks are tested according to the testing method of "Hazardous Waste Identification Standard - Leaching Toxicity Identification" (GBT2114-2007).

[0060] Six experiments were conducted for each example, and the experimental results were averaged over the six experiments.

[0061] The parameters of Examples 1-6 are shown in Table 1:

[0062] Table 1

[0063]

[0064]

[0065] The experimental results are shown in Table 2:

[0066] Table 2

[0067]

[0068] In summary, the various indicators of the electrolytic manganese slag prepared by the preparation method of the electrolytic manganese slag brick provided by the present invention meet the existing national standards, reducing damage to the environment while realizing resource reuse. Moreover, compared with the existing method, when using electrolytic manganese slag as a raw material for brick making, the ratio of electrolytic manganese slag can be increased, thereby increasing the consumption of electrolytic manganese slag. In the process of brick making, by treating ammonia nitrogen substances and solidifying manganese ions, the situation of manganese freedom and escape can be reduced, thereby reducing the adverse effects on the outside.

[0069] In the description of this specification, the description with reference to the terms "preferred embodiment", "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0070] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A method for preparing electrolytic manganese slag bricks, characterized in that: The following steps are involved: Step 1: ball-milling electrolytic manganese slag with magnesium oxide, calcium oxide and water to obtain a preliminary mixture, and then calcining to obtain material A for standby use; the weight ratio of electrolytic manganese slag, magnesium oxide, calcium oxide and water is 7-9:1:1.5:5; the calcination temperature is 700-900°C, and the calcination time is 30-90min; Step 2: Grind material A, and then filter out electrolytic manganese slag powder below 150 mesh for later use; Step 3: mixing electrolytic manganese slag powder, clay, ceramsite, cement and water in a weight ratio of 5:1:1:1:1-2, and mixing them evenly to form a green body; Step 4: preheating the green brick and then firing it to obtain electrolytic manganese slag brick; In step 1, pyrite is added during ball milling, and the weight ratio of pyrite to electrolytic manganese slag is 1:14-18; in step 3, lime is also included, and the weight ratio of lime to electrolytic manganese slag powder is 1:15; in step 4, three-stage firing is performed; In step 4, the firing temperature of the first stage is 800~950℃, and the firing time is 20~40min; the firing temperature of the second stage is 950~1100℃, and the firing time is 40~80min; the firing temperature of the third stage is 1100~1300℃, and the firing time is 30~60min.

2. The method for preparing an electrolytic manganese slag brick according to claim 1, characterized in that: In step 4, during preheating, the temperature is increased at a rate of 5°C / min until the temperature reaches 250~400°C, and preheated at this temperature for 30~50min.

Citation Information

Patent Citations

  • Method for extracting ammonium and modifying electrolytic manganese residue

    CN104529196A

  • Method and system for recovering electrolytic manganese slag

    CN104555947A

  • Electrolytic manganese residue sintered brick and preparation method thereof

    CN115028434A