Mosquito repellent composition, wall mosquito repellent coating, preparation method and use thereof

By combining permethrin and dextrotrans chloropropylenethrin with silicone surface additives and inorganic materials, a mosquito repellent composition is formed, which solves the problem of insufficient mosquito repellent effect and durability in wall coatings, and achieves the Efficient mosquito repellent effect and long-term mosquito repellent effect.

CN116855138BActive Publication Date: 2024-11-08FOSHAN DONGPENG CERAMIC +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310819013.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-05
Publication Date
2024-11-08
Estimated Expiration
2043-07-05

AI Technical Summary

Technical Problem

The adhesion effect of mosquito repellent in existing wall coatings is insufficient, and the mosquito repellent is poor, so it cannot effectively repel mosquitoes for a long time.

Method used

Component A and component B are used in combination, which contains permethrin and dextrotrans chloropropylene as the main mosquito repellent components, and is combined with silicone surface additive Byk-375 and component B The 98A acrylic emulsion curing reaction combines diatomaceous earth and inorganic materials to form a mosquito repellent composition, enhancing mosquito repellent effect and durability.

Benefits of technology

The mosquito repellent rate has reached 75%, which has significantly improved the mosquito repellent effect and durability, and solved the problem of insufficient mosquito repellent effect or poor durability in existing paints.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A mosquito repellent composition, a wall mosquito repellent coating, a preparation method and uses thereof; the mosquito repellent composition comprises component A and component B; component A and component B are mixed in a mass ratio of 1:(1-10); component A, its raw materials include: diatomaceous earth, permethrin, dextrorotatory trans-chlorprophmethrin, silicone surface additives Byk-375, Byk-P104S, Byk-80, polyether-modified polysiloxane solution Byk-20, leveling agent Byk-333 and water; component B, its raw materials include: BA101 titanium dioxide, talcum powder, calcium carbonate, methyl cellulose slurry, alcohol ester-12 film-forming aid, 98A acrylic emulsion, thickener, surface additive and water. A preparation method is used to prepare the above-mentioned mosquito repellent composition. This solution solves the problem that the existing coating has insufficient mosquito repellent effect or poor mosquito repellent durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mosquito repellent coatings, and in particular to a mosquito repellent composition, a wall mosquito repellent coating, a preparation method and uses thereof. Background Art

[0002] For the walls of kitchens or bathrooms, stagnant water in the environment is prone to breed mosquitoes, and users generally use mosquito coils, insecticides, mosquito-killing lamps and other methods to deal with them; but the mosquito repellent effect is poor; the existing technology is to directly add mosquito repellent to the paint, and then apply the paint to the surface of the tile, but the mosquito repellent effect of the paint is reduced; in particular, the adhesion effect of the paint on the mosquito repellent is insufficient, and the mosquito repellent has poor durability and is not suitable for long-term mosquito repellent. Summary of the invention

[0003] The object of the present invention is to provide a mosquito repellent composition, which is prepared by combining component A and component B, wherein the permethrin and dextrorotatory trans-chlorprophthrin in component A are used as main mosquito repellent components, and a silicone surface additive Byk-375 is cured with a 98A acrylic emulsion in component B to form a mosquito repellent component combined with a polymer structure, and diatomaceous earth and an inorganic material in the composition are combined, so that the mosquito repellent composition has excellent mosquito repellent effect and mosquito repellent durability.

[0004] The present invention also provides a method for preparing a mosquito repellent composition, which is used for preparing the above-mentioned mosquito repellent composition.

[0005] The present invention also provides a wall mosquito repellent coating using the above mosquito repellent composition.

[0006] The invention also provides a use of the composition in preparing mosquito repellent paint for walls.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] A mosquito repellent composition, comprising component A and component B;

[0009] The component A and the component B are mixed in a mass ratio of 1:(1-10);

[0010] The raw materials of component A include, by weight: 20-40 parts of diatomaceous earth, 0.1-2 parts of permethrin, 0.1-2 parts of dextrorotatory trans-chlorprophthrin, 0.1-2 parts of organosilicon surface additive Byk-375, 0.1-2 parts of Byk-P104S, 0.1-2 parts of Byk-80, 0.1-2 parts of polyether modified polysiloxane solution Byk-20, 0.1-2 parts of leveling agent Byk-333 and 50-100 parts of water;

[0011] The raw materials of component B include, by weight: 2-10 parts of BA101 titanium dioxide, 1-5 parts of talc, 10-30 parts of calcium carbonate, 2-8 parts of methyl cellulose pulp, 0.1-1.5 parts of alcohol ester-12 film-forming aid, 10-20 parts of 98A acrylic emulsion, 0.1-0.5 parts of thickener, 0.1-0.5 parts of surface additive and 20-50 parts of water.

[0012] Preferably, in the component B, the surface additive includes at least one or a combination of two or more of SN 5040 dispersant, NX2 defoamer and AMP-95 pH regulator.

[0013] A method for preparing a mosquito repellent composition, used for preparing the above-mentioned mosquito repellent composition, characterized in that component A and component B are stirred and mixed in proportion;

[0014] The preparation method of component A is as follows: the raw materials of component A are put into a reactor and stirred evenly, and then 0.1-5% of the total mass of an emulsifier is added, the speed of the reactor is set to 300-600 rpm, and the emulsification time is 5-20 min;

[0015] The preparation method of component B comprises the following steps:

[0016] (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm;

[0017] (2) adding a portion of the surface additive, methyl cellulose slurry and water under stirring;

[0018] (3) adding alcohol ester-12 film-forming aid under stirring conditions;

[0019] (4) Add 98A acrylic emulsion under stirring;

[0020] (5) Add thickener and water to adjust the viscosity.

[0021] A mosquito repellent paint for a wall uses the mosquito repellent composition mentioned above.

[0022] A use of a composition in preparing a wall mosquito repellent coating, wherein the composition is the above-mentioned mosquito repellent composition.

[0023] The technical solution provided by the present invention may include the following beneficial effects:

[0024] The present invention provides a mosquito repellent composition, which is prepared by combining component A and component B, wherein the permethrin and dextrorotatory trans-chlorprophmethrin in component A are used as main mosquito repellent components, and then the organosilicon surface additive Byk-375 is cured with the 98A acrylic emulsion in component B to form a mosquito repellent component combined with a polymer structure, and the diatomaceous earth and inorganic materials in the composition are combined, so that the mosquito repellent composition has excellent mosquito repellent effect and mosquito repellent durability, and the mosquito repellent rate reaches 75%, thereby solving the problem of insufficient mosquito repellent effect or poor mosquito repellent durability in existing coatings. DETAILED DESCRIPTION

[0025] The technical solution of this solution is further explained below through specific implementation methods.

[0026] A mosquito repellent composition, comprising component A and component B;

[0027] The component A and the component B are mixed in a mass ratio of 1:(1-10);

[0028] The raw materials of component A include, by weight: 20-40 parts of diatomaceous earth, 0.1-2 parts of permethrin, 0.1-2 parts of dextrorotatory trans-chlorprophthrin, 0.1-2 parts of organosilicon surface additive Byk-375, 0.1-2 parts of Byk-P104S, 0.1-2 parts of Byk-80, 0.1-2 parts of polyether modified polysiloxane solution Byk-20, 0.1-2 parts of leveling agent Byk-333 and 50-100 parts of water;

[0029] The raw materials of component B include, by weight: 2-10 parts of BA101 titanium dioxide, 1-5 parts of talc, 10-30 parts of calcium carbonate, 2-8 parts of methyl cellulose pulp, 0.1-1.5 parts of alcohol ester-12 film-forming aid, 10-20 parts of 98A acrylic emulsion, 0.1-0.5 parts of thickener, 0.1-0.5 parts of surface additive and 20-50 parts of water.

[0030] The present invention provides a mosquito repellent composition, which is prepared by combining component A and component B, wherein the permethrin and dextrorotatory trans-chlorprophmethrin in component A are used as main mosquito repellent components, and then the organosilicon surface additive Byk-375 is cured with the 98A acrylic emulsion in component B to form a mosquito repellent component combined with a polymer structure, and the diatomaceous earth and inorganic materials in the composition are combined, so that the mosquito repellent composition has excellent mosquito repellent effect and mosquito repellent durability, and the mosquito repellent rate reaches 75%, thereby solving the problem of insufficient mosquito repellent effect or poor mosquito repellent durability in existing coatings.

[0031] Preferably, in the component B, the surface additive includes at least one or a combination of two or more of SN 5040 dispersant, NX2 defoamer and AMP-95 pH regulator.

[0032] A method for preparing a mosquito repellent composition, used for preparing the above-mentioned mosquito repellent composition, characterized in that component A and component B are stirred and mixed in proportion;

[0033] Preparation method of component A: weigh the materials according to the proportion of component A, put them into the reactor and stir them evenly, then add 1% emulsifier of the total weight, set the reactor speed to 400 rpm, and the emulsification time to 5-20 min;

[0034] The preparation method of component B comprises the following steps:

[0035] (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm;

[0036] (2) adding a portion of the surface additive, methyl cellulose slurry and water under stirring;

[0037] (3) adding alcohol ester-12 film-forming aid under stirring conditions;

[0038] (4) Add 98A acrylic emulsion under stirring;

[0039] (5) Add thickener and water to adjust the viscosity.

[0040] A mosquito repellent paint for a wall uses the mosquito repellent composition mentioned above.

[0041] A use of a composition in preparing a wall mosquito repellent coating, wherein the composition is the above-mentioned mosquito repellent composition.

[0042] Performance Test:

[0043] Repellent rate: A homemade plexiglass testing device is made with live mosquitoes placed in it. The middle of the device is divided into left and right independent spaces, and a channel connecting the two independent spaces is opened in the middle. Before the test, mosquito repellent products are placed in one of the independent spaces, along with active mosquitoes. After one day, the number of remaining mosquitoes in the mosquito repellent product is observed, and the mosquito avoidance rate is calculated.

[0044] Repellency level: Tested according to the national standard GB / T13917-9-2009, Part 9 of Indoor Efficacy Test and Evaluation of Public Health Insecticides for Pesticide Registration.

[0045] Mosquito repellent durability: The mosquito repellent composition was applied to a plate exposed to air, and the mosquito repellency was tested every 10 days, and the number of days required for the mosquito repellency to be below 50% was recorded.

[0046] Embodiment A, including embodiments A1-A4;

[0047] In Example A, component A and component B are stirred and mixed according to the mass in Table 1;

[0048] Component A, in parts by mass, comprises: 38.15 parts of diatomaceous earth, 0.8 parts of permethrin, 0.25 parts of dextrorotatory trans-chlorpropethrin, 0.2 parts of organosilicon surface additive Byk-375, 0.2 parts of Byk-P104S, 0.1 parts of Byk-80, 0.1 parts of polyether modified polysiloxane solution Byk-20, 0.1 parts of leveling agent Byk-333 and 60 parts of water;

[0049] Preparation method of component A: weigh the materials according to the proportion of component A, put them into the reactor and stir them evenly, then add 1% emulsifier of the total weight, set the reactor speed to 400 rpm, and the emulsification time to 5 min;

[0050] Component B, by mass, includes: 8 parts of BA101 titanium dioxide, 5 parts of talc, 20 parts of calcium carbonate, 6 parts of methyl cellulose pulp, 1 part of alcohol ester-12 film-forming aid, 15 parts of 98A acrylic emulsion, 0.5 parts of thickener, 0.5 parts of surface additive and 35 parts of water; among the surface additives, SN 5040 dispersant, NX2 defoamer and AMP-95 pH regulator are prepared in a mass ratio of 1:2:2;

[0051] The preparation method of component B comprises the following steps:

[0052] (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm;

[0053] (2) adding a portion of the surface additive, methyl cellulose slurry and water under stirring;

[0054] (3) adding alcohol ester-12 film-forming aid under stirring conditions;

[0055] (4) Add 98A acrylic emulsion under stirring;

[0056] (5) Add thickener and water to adjust the viscosity.

[0057] The performance of Example A was tested, and the results are shown in Table 2.

[0058] Table 1 - Proportions of Component A and Component B of Example A

[0059] Components Example A1 Example A2 Example A3 Example A4 Component A (kg) 0.1 0.1 0.1 0 Component B (kg) 1 0.4 0.1 1

[0060] Table 2 - Performance comparison of Example A

[0061] Test items Example A1 Example A2 Example A3 Example A4 Mosquito repellent rate (%) 70 75 70 0 National standard grade Level A Level A Level A Failure Mosquito repellent durability (days) >180 >180 >180 0

[0062] illustrate:

[0063] 1. By comparing Examples A1-A3, it can be seen that the mass ratio of component A to component B in Example A1 is 1:10, the mass ratio of component A to component B in Example A2 is 1:4, and the mass ratio of component A to component B in Example A3 is 1:1. The mass ratios of Examples A1-A3 are all 1:(1-10), the mosquito repellent rates are all stable at 70-75%, the national standard grade is A, and the mosquito repellent durability can be greater than 180 days, indicating that controlling the mass ratio of component A to component B at 1:(1-10) can ensure the mosquito repellent rate and mosquito repellent durability.

[0064] 2. By comparing Example A1 and Example A4, it can be seen that Example A4 does not add component A, while component A contains mosquito repellent active ingredients such as permethrin and dextrorotatory trans-chlorpropynyl thrin, as well as silicone surface additive Byk-375. The silicone surface additive Byk-375 can react with the acrylic emulsion in component B during the coating curing reaction, so that the effective mosquito repellent component is combined in the polymer structure, so that the mosquito repellent efficiency is improved and the durability is enhanced. At the same time, diatomaceous earth has a certain porous structure, which can increase the specific surface area of ​​the material and better absorb the mosquito repellent component. Therefore, Example A4 does not have a mosquito repellent effect and mosquito repellent durability.

[0065] Embodiment B, including embodiments B1-B5;

[0066] In Example B, component A and component B are stirred and mixed at a mass ratio of 1:4;

[0067] Preparation method of component A, preparation method of component A, weigh the materials according to the proportion of component A, put them into the reactor and stir them evenly, then add 5% emulsifier of the total weight, set the reactor speed to 500 rpm, and the emulsification time to 10 min; the ingredients of component A are shown in Table 3;

[0068] Component B, by mass, includes: 8 parts of BA101 titanium dioxide, 5 parts of talc, 20 parts of calcium carbonate, 6 parts of methyl cellulose pulp, 1 part of alcohol ester-12 film-forming aid, 15 parts of 98A acrylic emulsion, 0.5 parts of thickener, 0.5 parts of surface additives and 20 parts of water. Among the surface additives, SN 5040 dispersant and AMP-95 pH regulator are added in a mass ratio of 3:2;

[0069] The preparation method of component B comprises the following steps:

[0070] (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm;

[0071] (2) adding a portion of the surface additive, methyl cellulose slurry and water under stirring;

[0072] (3) adding alcohol ester-12 film-forming aid under stirring conditions;

[0073] (4) Add 98A acrylic emulsion under stirring;

[0074] (5) Add thickener and water to adjust the viscosity.

[0075] Table 3 - Component A Ingredients for Example B

[0076] Components (parts) Example B1 Example B2 Example B3 Example B4 Example B5 diatomite 38 38 38 38 38 Permethrin 0.8 0 0.8 0.8 0.8 D-trans-chlorpromazine 0.25 0.25 0 0.25 0.25 Byk-375 0.2 0.2 0.2 0 0.2 Byk-P104S 0.2 0.2 0.2 0.2 0 Byk-80 0.1 0.1 0.1 0.1 0 Byk-20 0.1 0.1 0.1 0.1 0 Byk-333 0.1 0.1 0.1 0.1 0.1 water 60 60 60 60 60

[0077] Note: The raw materials in this table use brand names as abbreviations.

[0078] The performance of Examples B1-B5 was tested, and the results are shown in Table 4.

[0079] Table 4 - Performance Tests of Example B

[0080] Test items Example B1 Example B2 Example B3 Example B4 Example B5 Mosquito repellent rate (%) 75 55 60 60 70 National standard grade Level A Class B Class B Class B Level A Mosquito repellent durability (days) >180 30 50 50 30

[0081] illustrate:

[0082] 1. By comparing Example B1, Example B2 and Example B3, it can be seen that Example B2 does not add chlorfenapyr, which results in the mosquito repellent rate of Example B2 being only 55%, and the national standard grade is B; and because its own mosquito repellent rate base is low, its own mosquito repellent durability is insufficient. Example B3 does not add dextrorotatory trans-chlorfenapyr, which results in the mosquito repellent rate of Example B3 being 60%, and the national standard grade is B; while Example B1 uses chlorfenapyr and dextrorotatory trans-chlorfenapyr in combination, and through the added silicone surface additive and the 98A acrylic emulsion of component B, chlorfenapyr and dextrorotatory trans-chlorfenapyr react with the acrylic emulsion in component B during the coating curing reaction, so that the effective mosquito repellent component is combined in the polymer structure, so that the mosquito repellent efficiency is improved and the durability is enhanced. Therefore, the mosquito repellent rate of Example B1 can reach 75%, the national standard grade is A, and the mosquito repellent durability is greater than 180 days. It is explained that both permethrin and d-trans-chlorpropynyl can be combined with silicone surface additives and 98A acrylic emulsion of component B to further improve the mosquito repellency rate and mosquito repellency durability.

[0083] 2. By comparing Example B1 with Example B4, it can be seen that Example B4 does not add Byk-375. Here, Byk-375 is an organosilicon surface additive Byk-375. The organosilicon surface additive Byk-375 can effectively cooperate with the 98A acrylic emulsion of component B, thereby improving the mosquito repellency and mosquito repellency durability of both permethrin and d-trans-chlorpropylthrin. However, Example B4 does not add Byk-375, resulting in the mosquito repellency of Example B4 dropping to 60%, and the mosquito repellency durability is only 50 days.

[0084] 3. By comparing Example B1 with Example B5, it can be seen that Example B5 does not add Byk-P104S, Byk-80 and Byk-20, which are Byk-P104S, Byk-P104S and polyether-modified polysiloxane solution Byk-20, respectively. The three can assist in emulsifying permethrin and dextrorotatory trans-chlorpropargyl thrin and dispersing them in the water of component B. After component A and component B are made into a coating, the dispersed permethrin and dextrorotatory trans-chlorpropargyl thrin can be fixed on the outer surface of the object, and permethrin and dextrorotatory trans-chlorpropargyl thrin can be slowly released, thereby improving the mosquito repellent durability. Although Example B5 has a mosquito repellent effect of 70%, its mosquito repellent durability is reduced.

[0085] Example C:

[0086] In Example C, component A and component B are stirred and mixed at a mass ratio of 1:5;

[0087] Component A, in parts by mass, comprises: 38.15 parts of diatomaceous earth, 0.8 parts of permethrin, 0.25 parts of dextrorotatory trans-chlorpropethrin, 0.2 parts of organosilicon surface additive Byk-375, 0.2 parts of Byk-P104S, 0.1 parts of Byk-80, 0.1 parts of polyether modified polysiloxane solution Byk-20, 0.1 parts of leveling agent Byk-333 and 80 parts of water;

[0088] Preparation method of component A: weigh the materials according to the proportion of component A, put them into the reactor and stir them evenly, then add 1% emulsifier of the total weight, set the reactor speed to 600 rpm, and the emulsification time to 10 min;

[0089] The ingredients of component B are shown in Table 5; the preparation method of component B comprises the following steps:

[0090] (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm;

[0091] (2) adding a portion of the surface additive, methyl cellulose slurry and water under stirring; the surface additive is NX2 defoamer;

[0092] (3) adding alcohol ester-12 film-forming aid under stirring conditions;

[0093] (4) Add 98A acrylic emulsion under stirring;

[0094] (5) Add thickener and water to adjust the viscosity.

[0095] Table 5 - Component B Ingredients of Example C

[0096] Components (parts) Example C1 Example C2 Example C3 BA101 Titanium Dioxide 8 8 0 talcum powder 5 5 0 Calcium carbonate 20 20 0 Methylcellulose pulp 6 6 6 Alcohol ester-12 film-forming aid 1 1 1 98A acrylic emulsion 15 0 15 Thickener 0.5 0.5 0.5 Surface additives 0.5 0.5 0.5 water 30 45 30

[0097] The performance of Example C was tested, and the results are shown in Table 6.

[0098] Table 6 - Performance Tests of Example C

[0099] Test items Example C1 Example C2 Example C3 Mosquito repellent rate (%) 75 60 70 National standard grade Level A Class B Level A Mosquito repellent durability (days) >180 50 50

[0100] illustrate:

[0101] 1. By comparing Example C1 with Example C2, it can be seen that Example C2 does not add 98A acrylic emulsion, and 15 parts of water are used to replace the 98A acrylic emulsion in Example C1; while in this scheme, the silicone surface additive Byk-375 reacts with the 98A acrylic emulsion during the coating curing reaction, so that the effective mosquito repellent component is combined with the polymer structure, so that the mosquito repellent efficiency is improved and the durability is enhanced. Therefore, Example C2 does not form an internal cross-adhesive structure, resulting in the failure of the effective mosquito repellent component to be combined with the polymer structure, and the adhesion effect of the effective mosquito repellent component is insufficient. On the one hand, it is easy to fall off, affecting the mosquito repellent effect and mosquito repellent durability; on the other hand, since the 98A acrylic emulsion forms multiple microporous structures on the surface after the water evaporates, it can be combined with diatomaceous earth to improve the slow release effect of the effective mosquito repellent component.

[0102] 2. By comparing Examples C1 and C3, it can be seen that Example C3 does not add BA101 titanium dioxide, talcum powder and calcium carbonate as inorganic materials, while the inorganic materials in this application have the function of increasing whiteness and viscosity, which can be more convenient for construction, and can be combined with diatomaceous earth to physically adsorb the mosquito repellent, thereby increasing the service life of the mosquito repellent. Therefore, the mosquito repellent durability of Example C3 decreases, indicating that adding BA101 titanium dioxide, talcum powder and calcium carbonate as inorganic materials can improve the durability of the mosquito repellent.

[0103] Embodiment D:

[0104] In Example D, component A and component B are stirred and mixed at a mass ratio of 1:4;

[0105] Component A, in parts by mass, comprises: 20 parts of diatomaceous earth, 2 parts of permethrin, 2 parts of dextro-trans-chlorprophthrin, 2 parts of organosilicon surface additive Byk-375, 2 parts of Byk-P104S, 2 parts of Byk-80, 2 parts of polyether modified polysiloxane solution Byk-20, 2 parts of leveling agent Byk-333 and 100 parts of water;

[0106] Preparation method of component A: weigh the materials according to the proportion of component A, put them into the reactor and stir them evenly, then add 1% emulsifier of the total weight, set the reactor speed to 300 rpm, and the emulsification time to 5 min;

[0107] Component B, its raw materials include, by mass: 2 parts of BA101 titanium dioxide, 1 part of talc, 30 parts of calcium carbonate, 2 parts of methyl cellulose pulp, 0.1 parts of alcohol ester-12 film-forming aid, 20 parts of 98A acrylic emulsion, 0.1 parts of thickener, 0.1 parts of surface additives and 35 parts of water; among the surface additives, SN 5040 dispersant, NX2 defoamer and AMP-95 pH regulator are prepared in a mass ratio of 1:1:3;

[0108] The preparation method of component B comprises the following steps:

[0109] (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm;

[0110] (2) adding a portion of the surface additive, methyl cellulose slurry and water under stirring;

[0111] (3) adding alcohol ester-12 film-forming aid under stirring conditions;

[0112] (4) Add 98A acrylic emulsion under stirring;

[0113] (5) Add thickener and water to adjust the viscosity.

[0114] Embodiment E:

[0115] In Example E, component A and component B are stirred and mixed at a mass ratio of 1:5;

[0116] Component A, in parts by mass, comprises: 40 parts of diatomaceous earth, 0.1 parts of permethrin, 0.1 parts of dextrorotatory trans-chlorpropethrin, 2 parts of silicone surface additive Byk-375, 0.1 parts of Byk-P104S, 2 parts of Byk-80, 0.1 parts of polyether modified polysiloxane solution Byk-20, 0.1 parts of leveling agent Byk-333 and 50 parts of water;

[0117] Preparation method of component A: weigh the materials according to the proportion of component A, put them into the reactor and stir them evenly, then add 3% emulsifier of the total weight, set the reactor speed to 600 rpm, and the emulsification time to 5 min;

[0118] Component B, its raw materials include, by mass: 10 parts of BA101 titanium dioxide, 5 parts of talc, 10 parts of calcium carbonate, 8 parts of methyl cellulose pulp, 1.5 parts of alcohol ester-12 film-forming aid, 10 parts of 98A acrylic emulsion, 0.5 parts of thickener, 0.5 parts of surface additive and 50 parts of water; among the surface additives, SN 5040 dispersant, NX2 defoamer and AMP-95 pH regulator are prepared in a mass ratio of 0.5:1.5:3;

[0119] The preparation method of component B comprises the following steps:

[0120] (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm;

[0121] (2) adding a portion of the surface additive, methyl cellulose slurry and water under stirring;

[0122] (3) adding alcohol ester-12 film-forming aid under stirring conditions;

[0123] (4) Add 98A acrylic emulsion under stirring;

[0124] (5) Add thickener and water to adjust the viscosity.

[0125] The performance of Examples D and E was tested, and the results are shown in Table 7.

[0126] Table 7 - Performance Tests of Examples D and E

[0127] Test items Example D Example E Mosquito repellent rate (%) 71 73 National standard grade Level A Level A Mosquito repellent durability (days) >180 >180

[0128] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the protection scope of the present invention in any way. Based on the explanations herein, those skilled in the art can think of other specific implementation methods of the present invention without creative work, and these methods will fall within the protection scope of the present invention.

Claims

1. A mosquito repellent composition, characterized in that: Comprising component A and component B; The component A and the component B are mixed in a mass ratio of 1:(1-10); The raw materials of component A include, by weight: 20-40 parts of diatomaceous earth, 0.1-2 parts of permethrin, 0.1-2 parts of dextrorotatory trans-chlorprophthrin, 0.1-2 parts of organosilicon surface additive Byk-375, 0.1-2 parts of Byk-P104S, 0.1-2 parts of Byk-80, 0.1-2 parts of polyether modified polysiloxane solution Byk-20, 0.1-2 parts of leveling agent Byk-333 and 50-100 parts of water; The raw materials of component B include, by weight: 2-10 parts of BA101 titanium dioxide, 1-5 parts of talc, 10-30 parts of calcium carbonate, 2-8 parts of methyl cellulose pulp, 0.1-1.5 parts of alcohol ester-12 film-forming aid, 10-20 parts of 98A acrylic emulsion, 0.1-0.5 parts of thickener, 0.1-0.5 parts of surface additive and 20-50 parts of water; The preparation method of the mosquito repellent composition comprises mixing component A and component B in a certain proportion; The preparation method of component A is as follows: the raw materials of component A are put into a reactor and stirred evenly, and then 0.1-5% of the total mass of an emulsifier is added, and the speed of the reactor is set to 300-600 rpm, and the emulsification is completed to obtain the product; The preparation method of component B comprises the following steps: (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm; (2) adding part of the surface additive, methyl cellulose slurry and water under stirring; (3) Adding alcohol ester-12 film-forming aid under stirring conditions; (4) Add 98A acrylic emulsion under stirring conditions; (5) Add thickener and water to adjust viscosity; The surface additive includes at least one of SN 5040 dispersant, NX2 defoamer and AMP-95 pH adjuster.

2. A method for preparing a mosquito repellent composition, for preparing a mosquito repellent composition according to claim 1, characterized in that: Mix component A and component B in proportion; The preparation method of component A is as follows: the raw materials of component A are put into a reactor and stirred evenly, and then 0.1-5% of the total mass of an emulsifier is added, and the speed of the reactor is set to 300-600 rpm, and the emulsification is completed to obtain the product; The preparation method of component B comprises the following steps: (1) Mix BA101 titanium dioxide, talcum powder, calcium carbonate and some surface additives with water, mix well and grind to a fineness of less than 60 μm; (2) adding part of the surface additive, methyl cellulose slurry and water under stirring; (3) Adding alcohol ester-12 film-forming aid under stirring conditions; (4) Add 98A acrylic emulsion under stirring conditions; (5) Add thickener and water to adjust the viscosity.

3. A wall mosquito repellent paint, characterized in that: Use the mosquito repellent composition described in claim 1.

4. Use of a composition in preparing a wall mosquito repellent coating, characterized in that: The composition is a mosquito repellent composition as claimed in claim 1.