A thick high-nitrogen weather-resistant and earthquake-resistant H-shaped steel and its preparation method

By controlling the high nitrogen content in thick-gauge H-shaped steel and optimizing the chemical composition and production process, the problem of unstable low-temperature impact performance of thick-gauge H-shaped steel was solved, and thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel with high strength and excellent low-temperature impact toughness was achieved. The steel profiles are prepared to meet high performance and quality standards.

CN116891985BActive Publication Date: 2024-10-29BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310711729.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-15
Publication Date
2024-10-29
Estimated Expiration
2043-06-15

AI Technical Summary

Technical Problem

Thick H-shaped steel has poor low-temperature impact performance stability due to poor and uneven deformation during the rolling process, affecting its overall performance and quality improvement.

Method used

By controlling high nitrogen content and optimizing chemical composition and production process conditions, blast furnace molten iron pretreatment, converter smelting, LF refining, special-shaped billet continuous casting, walking heating furnace, high-pressure water phosphorus removal, BD billet opening, CCS universal rolling, etc. Process steps to ensure the low-temperature impact toughness performance of steel.

Benefits of technology

It has achieved excellent low-temperature impact toughness of thick-sized high-nitrogen weather-resistant and earthquake-resistant H-shaped steel. The mechanical properties have reached yield strength ≥449MPa, tensile strength ≥597MPa, elongation ≥23%, and average room temperature impact ≥133.2J. The stability and quality have reached standards. Require.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004288049200000041
    Figure BDA0004288049200000041
Patent Text Reader

Abstract

The invention discloses a thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel and a preparation method thereof, wherein the chemical composition of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel is calculated by mass percentage as follows: C 0.07%-0.10%, Si 0.50%-0.60%, Mn 1.40%-1.50%, P≤0.025%, S≤0.010%, Cr 0.30%-0.36%, Cu 0.25%-0.31%, Ni 0.25%-0.30%, V 0.14%-0.16%, N 0.020%-0.024%, and the balance is Fe and unavoidable impurities; the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel disclosed by the invention has excellent comprehensive mechanical properties, especially low-temperature impact toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of weathering steel production, and specifically relates to a thick-gauge high-nitrogen weathering and earthquake-resistant H-shaped steel with excellent low-temperature impact toughness and a preparation method thereof. Background Art

[0002] In microalloyed steel, the beneficial effect of nitrogen addition lies in its interaction with microalloying elements. Since the nitrides of microalloying elements are more stable than carbides and have a lower tendency to aggregate, increasing the nitrogen content will maximize the ratio of particle volume percentage to particle size. Therefore, the key to microalloyed steel is to maximize the microstructure, i.e., grain refinement and precipitation strengthening. Nitrogen has a significant effect on the precipitation phase of microalloyed steel. After nitrogen addition to the steel, the number of V (C, N) precipitation phases increases exponentially. In low-nitrogen vanadium steel, the weight fraction of V (C, N) precipitation phases is only 0.0498%, while in high-nitrogen vanadium steel, the weight fraction of V (C, N) precipitation phases reaches 0.1062%. Therefore, nitrogen greatly promotes the precipitation of vanadium in steel.

[0003] Nitrogen not only promotes the precipitation of vanadium in steel, but also changes the distribution of vanadium in the phases. In low-nitrogen steel, 56.3% of vanadium is dissolved in the matrix, and only 35.5% of vanadium is precipitated in the form of V (C, N), while 70.0% of vanadium in high-nitrogen steel is precipitated in the form of V (C, N), leaving only a small amount of vanadium dissolved in the matrix. A large number of studies have confirmed that increasing nitrogen in steel can save 20% to 40% of vanadium. Through theoretical analysis, it can be seen that the ideal chemical ratio of V and N in vanadium steel is 3.64, which is the mass ratio of V and N that produces maximum precipitation strengthening.

[0004] Due to the small rolling compression ratio and deformation of thick H-beams, the deformation permeability of H-beams of various specifications is poor during the rolling process, there are many uneven deformations, and the rolling temperature is high, resulting in poor stability of the low-temperature impact performance of the product and large fluctuations in the impact performance of different parts. Therefore, the mechanical properties of thick H-beams, especially the low-temperature impact performance, have become an important factor restricting the improvement of the overall performance, quality, and indicators of thick high-strength weather-resistant H-beams. Summary of the invention

[0005] In view of the problems existing in the prior art, one aspect of the present invention provides a thick-gauge high-nitrogen weathering and earthquake-resistant H-shaped steel, in particular a thick-gauge high-nitrogen weathering and earthquake-resistant H-shaped steel with excellent low-temperature impact toughness, wherein the chemical composition thereof is calculated by mass percentage as follows: C 0.07% to 0.10%, Si 0.50% to 0.60%, Mn 1.40% to 1.50%, P≤0.025%, S≤0.010%, Cr0.30% to 0.36%, Cu 0.25% to 0.31%, Ni 0.25% to 0.30%, V 0.14% to 0.16%, N 0.020% to 0.024%, and the balance is Fe and unavoidable impurities;

[0006] The mechanical properties of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel meet the following requirements: yield strength ≥449MPa, tensile strength ≥597MPa, elongation ≥23%, and average room temperature impact strength ≥133.2J.

[0007] In some embodiments, the chemical composition of the thick-gauge high-nitrogen weathering and earthquake-resistant H-shaped steel is calculated by mass percentage as follows: C 0.07% to 0.10%, Si 0.53% to 0.60%, Mn 1.40% to 1.49%, P≤0.015%, S≤0.010%, Cr 0.30% to 0.36%, Cu 0.29% to 0.31%, Ni 0.28% to 0.29%, V 0.14% to 0.16%, N0.020% to 0.024%, and the balance is Fe and unavoidable impurities.

[0008] In some embodiments, the size of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel is 618*306*18*35mm.

[0009] On the other hand, the present invention provides a method for preparing thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel, which comprises the following process steps: blast furnace molten iron - molten iron pretreatment - converter smelting - LF refining - special-shaped billet continuous casting - feeding - walking beam heating furnace - high-pressure water dephosphorization - BD billet opening - CCS universal rolling - hot sawing - walking beam cooling bed cooling - straightening - sawing; wherein:

[0010] During the molten iron pretreatment process, pre-treated desulfurized molten iron is used: [S] entering the converter is <0.030%; the molten iron temperature is greater than or equal to 1250°C.

[0011] In the converter smelting process, the combined blowing converter smelting controls the final slag basicity to 3.0, the end point C ≥ 0.03%, the end point temperature is greater than or equal to 1610°C, the final deoxidation adopts Al deoxidation, alloy copper and nickel are added with scrap steel, and lime is added during the steel tapping process;

[0012] During the LF refining process, the white slag is refined, and the Ar blowing operation is carried out according to the refining regulations. Desulfurization, composition fine-tuning and temperature-raising operations are carried out according to the composition and temperature of the molten steel in the converter. In the later stage of refining, 65kg / furnace of vanadium-nitrogen alloy is added. If the vanadium content is insufficient, ferrovanadium is used to supplement it, and the composition is fine-tuned. At the end of refining, 150m of silicon-calcium wire is fed to ensure that the soft blowing time is greater than or equal to 15min. The molten steel shall not be exposed during the soft blowing.

[0013] During the continuous casting of special-shaped billets, protective pouring, weak cooling system and constant casting speed are adopted throughout the process. After the continuous casting billets are cut, they are stacked and slowly cooled in time, and the cover mold is laid on the bottom. The slow cooling time is greater than or equal to 48 hours.

[0014] When heating the ingot, fast firing is adopted, and the reducing atmosphere in the furnace is ensured at the same time; the temperature of the preheating section is controlled at ≤1000℃, the temperature of the first heating section is controlled at ≤1200℃, the temperature of the second heating section is controlled at 1100-1330℃, the temperature of the soaking section is controlled at 1100-1330℃, and the total heating time of the ingot is controlled at 3-5h;

[0015] Before the ingot is put into BD1, it must be dephosphorized with high-pressure water to prevent the surface defects of the finished H-beam caused by the pressing of the iron oxide ingot;

[0016] The blanking mill is designed to roll 8 times, and the blanking area is not subjected to controlled rolling, and the rolling temperature is controlled at 1170-1190℃;

[0017] The CCS universal rolling mill is designed to roll 5 times and perform controlled rolling to produce sufficiently uniform deformation bands in the austenite crystals, nucleate ferrite in the crystals and on the deformation bands, refine the grains, and control the final rolling temperature at 960-995°C; control the upper cooling bed temperature of the finished H-beam to ≥850°C, and perform close cooling.

[0018] The advantages of the present invention are: the present invention provides a thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel with excellent low-temperature impact toughness, which can further improve the low-temperature impact toughness of the steel while ensuring or further optimizing the strength performance of the steel by controlling the high nitrogen content and optimizing the chemical composition content and production process conditions in the steel. The mechanical properties of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel with excellent low-temperature impact toughness provided by the present invention meet the following requirements: yield strength ≥449MPa, tensile strength ≥597MPa, elongation ≥23%, and room temperature impact average value ≥133.2J. DETAILED DESCRIPTION

[0019] The present invention is described in detail below through specific examples. The examples are intended to help understand the present invention but are not intended to limit the present invention.

[0020] Example: Preparation of a thick gauge high nitrogen weathering and earthquake resistant H-beam with excellent low temperature impact toughness

[0021] The method for preparing thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel with excellent low-temperature impact toughness provided in this embodiment comprises the following process steps: blast furnace molten iron - molten iron pretreatment - converter smelting - LF refining - special-shaped billet continuous casting - feeding - walking beam heating furnace - high-pressure water dephosphorization - BD billet opening - CCS universal rolling - hot sawing - walking beam cooling bed cooling - straightening - sawing; wherein:

[0022] During the molten iron pretreatment process, pre-treated desulfurized molten iron is used: [S] entering the converter is <0.030%; the molten iron temperature is greater than or equal to 1250°C.

[0023] In the converter smelting process, the combined blowing converter smelting controls the final slag basicity to 3.0, the end point C ≥ 0.03%, the end point temperature is greater than or equal to 1610°C, the final deoxidation adopts Al deoxidation, alloy copper and nickel are added with scrap steel, and lime is added during the steel tapping process;

[0024] During the LF refining process, the white slag is refined, and the Ar blowing operation is carried out according to the refining regulations. Desulfurization, composition fine-tuning and temperature-raising operations are carried out according to the composition and temperature of the molten steel in the converter. In the later stage of refining, 65kg / furnace of vanadium-nitrogen alloy is added. If the vanadium content is insufficient, ferrovanadium is used to supplement it, and the composition is fine-tuned. At the end of refining, 150m of silicon-calcium wire is fed to ensure that the soft blowing time is greater than or equal to 15min. The molten steel shall not be exposed during the soft blowing.

[0025] During the continuous casting of special-shaped billets, protective pouring, weak cooling system and constant casting speed are adopted throughout the process. After the continuous casting billets are cut, they are stacked and slowly cooled in time, and the cover mold is laid on the bottom. The slow cooling time is greater than or equal to 48 hours.

[0026] When heating the ingot, fast firing is adopted, and the reducing atmosphere in the furnace is ensured at the same time; the temperature of the preheating section is controlled at ≤1000℃, the temperature of the first heating section is controlled at ≤1200℃, the temperature of the second heating section is controlled at 1100-1330℃, the temperature of the soaking section is controlled at 1100-1330℃, and the total heating time of the ingot is controlled at 3-5h;

[0027] Before the ingot is put into BD1, it must be dephosphorized with high-pressure water to prevent the surface defects of the finished H-beam caused by the pressing of the iron oxide ingot;

[0028] The blanking mill is designed to roll 8 times, and the blanking area is not subjected to controlled rolling, and the rolling temperature is controlled at 1170-1190℃;

[0029] The CCS universal rolling mill is designed to roll 5 times and perform controlled rolling to produce sufficiently uniform deformation bands in the austenite crystals, nucleate ferrite in the crystals and on the deformation bands, refine the grains, and control the final rolling temperature at 960-995°C. The upper cooling bed temperature of the finished H-shaped steel is controlled to be ≥850°C, and close cooling is performed. The finished product size is 618*306*18*35mm.

[0030] Check the surface quality and overall dimensions of thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel.

[0031] No obvious surface defects of the finished product were found during the inspection. The external dimensions of the finished H-beam met the standard requirements, the surface quality was good, all properties of the H-beam after rolling met the standard requirements, and the room temperature impact toughness stability was good.

[0032] Table 1 below shows the chemical composition of the steel grades in each embodiment, Table 2 below shows the control conditions of the starting and final rolling temperatures in each embodiment, and Table 3 below shows the mechanical properties and grain size test results of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel prepared in the embodiment.

[0033] Table 1: Chemical composition of each example (mass percentage / %)

[0034] Example C Si Mn P S Cr Ni Cu V N 1 0.07 0.60 1.43 0.0109 0.007 0.354 0.285 0.292 0.150 0.020 2 0.08 0.57 1.40 0.0114 0.006 0.338 0.283 0.307 0.155 0.021 3 0.09 0.53 1.42 0.0111 0.008 0.36 0.281 0.306 0.154 0.023 4 0.10 0.53 1.49 0.009 0.006 0.34 0.288 0.296 0.148 0.024

[0035] Table 2: Starting and final rolling temperature control in various embodiments

[0036] Example Rolling temperature (℃) Finishing rolling temperature(℃) 1 1173 976 2 1178 972 3 1170 980 4 1180 979

[0037] Table 3 Mechanical properties and grain size of each embodiment

[0038]

[0039] It can be seen from the above embodiments that the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel prepared by the method of the present invention not only has high strength, but also has excellent and stable impact toughness.

[0040] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel, characterized in that: The chemical composition of the thick-gauge high-nitrogen weathering and earthquake-resistant H-shaped steel is as follows by mass percentage: C 0.10%, Si 0.53%, Mn 1.49%, P 0.009%, S 0.006%, Cr 0.34%, Cu 0.296%, Ni 0.288%, V 0.148%, N 0.024%, and the balance is Fe and unavoidable impurities; The mechanical properties of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel meet the following requirements: yield strength 481MPa, tensile strength 639MPa, elongation 23%, yield strength ratio 0.75, and room temperature impact average value 151.4J; The preparation method of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel comprises the following process steps: blast furnace molten iron - molten iron pretreatment - converter smelting - LF refining - special-shaped billet continuous casting - feeding - walking beam heating furnace - high-pressure water descaling - BD billet opening - CCS universal rolling - hot sawing - walking beam cooling bed cooling - straightening - sawing; wherein: In the process of hot metal pretreatment, pretreatment desulfurized hot metal is used: [S] < 0.030% when entering the converter; hot metal temperature is greater than or equal to 1250℃; During converter smelting, the combined blowing converter smelting controls the final slag basicity to 3.0, the end point C ≥ 0.03%, the end point temperature to be greater than or equal to 1610°C, the final deoxidation adopts Al deoxidation, alloy copper and nickel are added with scrap steel, and lime is added during the steelmaking process; During the LF refining process, the white slag is refined, and the Ar blowing operation is carried out according to the refining regulations. Desulfurization, composition fine-tuning and temperature-raising operations are carried out according to the composition and temperature of the molten steel in the converter. In the later stage of refining, 65kg / furnace of vanadium-nitrogen alloy is added. If the vanadium content is insufficient, ferrovanadium is used to supplement it, and the composition is fine-tuned. At the end of refining, 150m of silicon-calcium wire is fed to ensure that the soft blowing time is greater than or equal to 15min. The molten steel shall not be exposed during the soft blowing. During the continuous casting of special-shaped billets, protective pouring, weak cooling system and constant casting speed are adopted throughout the process. After the continuous casting billets are cut, they are stacked and slowly cooled in time, and the cover mold is laid on the bottom. The slow cooling time is greater than or equal to 48 hours. When heating the ingot, fast firing is adopted, and the reducing atmosphere in the furnace is ensured at the same time; the temperature of the preheating section is controlled at ≤1000℃, the temperature of the first heating section is controlled at ≤1200℃, the temperature of the second heating section is controlled at 1100-1330℃, the temperature of the soaking section is controlled at 1100-1330℃, and the total heating time of the ingot is controlled at 3-5h; Before the ingot enters BD1, it must be descaled with high-pressure water to prevent the surface defects of the finished H-beam caused by the pressure of oxidized iron scale; The blanking mill is designed to roll 8 times, and the blanking area is not subjected to controlled rolling, and the rolling temperature is controlled at 1180℃; The CCS universal rolling mill is designed to roll 5 times and perform controlled rolling to produce sufficiently uniform deformation bands in the austenite crystals, nucleate ferrite in the crystals and on the deformation bands, refine the grains, and control the final rolling temperature at 979°C; control the upper cooling bed temperature of the finished H-beam to ≥850°C, and perform close cooling.

2. The thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel according to claim 1 is characterized in that: The size of the thick-gauge high-nitrogen weather-resistant and earthquake-resistant H-shaped steel is 618*306*18*35mm.

Citation Information

Patent Citations

  • Thick-specification high-strength weather-resistant anti-seismic H-shaped steel and rolling method thereof

    CN115354222A

  • Thick-specification high-strength weather-resistant anti-seismic hot-rolled H-shaped steel for building steel structure

    CN115725901A

  • Smelting method of thick-specification high-strength weather-resistant anti-seismic H-shaped steel

    CN116065083A

  • V-series 550MPa-grade anti-seismic weather-resistant steel plate for building structure and preparation method thereof

    CN116083792A