A preparation method of composite copper foil and composite copper foil

By employing a combination of amorphous silicon film, flexible substrate film, and copper film in composite copper foil, and using laser irradiation to achieve non-destructive peeling, the tearing problem of composite metal foil during peeling from the substrate is solved, and a thinner composite copper foil with stable performance is prepared.

CN116892000BActive Publication Date: 2024-11-01ANHUI LUMITO ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310850248.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-11
Publication Date
2024-11-01
Estimated Expiration
2043-07-11

AI Technical Summary

Technical Problem

In the prior art, composite metal foils are prone to tearing the flexible substrate layer when peeled off from the substrate, resulting in damage to the performance of the metal foil. Furthermore, high-energy laser peeling can easily damage the film structure, making it difficult to select a suitable laser for peeling.

Method used

A composite structure consisting of an amorphous silicon film, a flexible substrate film, and a copper film is adopted. By coating the amorphous silicon film with the flexible substrate film and the copper film, and using laser irradiation to separate the amorphous silicon film from the substrate, the hydrogen content of the amorphous silicon film and the laser parameters are controlled to achieve non-destructive peeling.

Benefits of technology

This method enables the composite copper foil to be easily peeled off from the substrate without damaging the film structure, resulting in a uniform and stable film layer, and allows for the preparation of thinner composite copper foils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116892000B_ABST
    Figure CN116892000B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite copper foil and a composite copper foil, comprising an amorphous silicon film layer, a flexible base film layer, and a copper film layer. The amorphous silicon film layer is plated on one surface of a high temperature resistant base material, hydrogenated, a flexible base film layer is coated on the amorphous silicon film layer, and a copper film layer is plated on the flexible base film layer to form a composite copper foil. Under laser irradiation, the amorphous silicon film layer is peeled off from the base material to obtain a composite copper foil. The composite copper foil has a uniform film layer and is easy to peel off from the base material. The film layer structure of the composite copper foil will not be damaged during peeling, and the integrity of the film layer can be well maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of batteries, and in particular to a preparation method of a composite copper foil and the composite copper foil. Background Art

[0002] Metal foil is usually used as a current collector for lithium batteries. The material of the metal foil is mostly selected from copper or aluminum. In order to improve the mechanical properties of the metal foil and enhance the impact resistance of the metal foil, a composite metal foil is provided in the prior art. A flexible substrate layer is designed under the metal layer of the composite metal foil to enhance the overall flexibility. For industrial application and cost reduction considerations, it is hoped to produce a composite metal foil that is thinner than the prior art. However, the ultra-thin composite metal foil is prone to wrinkles during the preparation process and needs to be fixed on a certain substrate for processing. After the processing is completed, it is peeled off. In the prior art, when the metal foil is peeled off from the substrate, it is easy to tear the flexible substrate layer, thereby damaging the performance of the metal foil. If the entire metal foil is to be completely peeled off, a laser with higher energy needs to be selected. However, a high-energy laser is also easy to damage the film layer. There are certain difficulties in selecting a laser that can peel off the metal foil without damaging the film layer structure. Therefore, it is a problem that the prior art needs to solve to manufacture a composite metal foil that is easy to peel off from a substrate. The present invention provides a composite metal foil that is easy to peel off from a substrate.

[0003] The Chinese patent document with the publication number CN115224282A discloses a method for preparing a plastic composite conductive film for an aluminum ion battery positive electrode current collector, wherein conductive carbon is uniformly dispersed in a first solution to form a second solution with a conductive carbon concentration of 5-30 g / mL, the second solution is uniformly coated on an easily peelable substrate by a coating method, and the plastic composite conductive film is obtained by peeling after being placed in an oven for drying, wherein the first solution is a polymer solution formed by dissolving a polymer in a solvent, the mass percentage content of the conductive carbon in the plastic composite conductive film is 5% to 99%, the mass percentage content of the polymer is 0% to 90%, the conductivity of the aluminum ion battery conductive carbon / polymer current collector is 150-104 Scm-1, and the thickness is 50-1000 microns, and the invention also relates to the application of the plastic composite conductive film. In this invention, the conductive material is directly coated on the substrate, and the composite conductive film is easily damaged during peeling, causing the conductive film to tear.

[0004] The Chinese patent document with publication number CN114284505A discloses a porous copper current collector and its preparation method and application in zinc / sodium ion batteries. This invention uses bronze alloy as raw material. The bronze alloy is a copper-tin alloy with a high tin content. Tin has a relatively unique property and has good affinity with most metal negative electrodes. It can be used as a nucleating agent to induce uniform deposition and growth of metals. However, the inventors have found that it is difficult to induce uniform deposition of metallic zinc by directly using bronze alloy. Therefore, the present invention adopts an electrochemical dealloying method under acidic conditions for preparation, which can regulate the micromorphology and tin content in the bronze alloy, thereby inducing uniform deposition of metallic zinc and improving the deposition and stripping efficiency of zinc. In addition, tin has a high metallic activity and can directly react with hydrogen ions. In order to improve the control of the tin content in the porous copper current collector, the present invention adopts a specific acid and concentration to ensure the control of the tin content in the porous copper current collector. This invention uses uniform deposition of a metal film layer to improve the stripping efficiency, but this method cannot improve the stripping efficiency well. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing a composite copper foil and a composite copper foil. The composite copper foil prepared by this method is easy to peel off from a substrate without destroying the composite film layer structure during peeling, and the film layer is uniform and the composite copper foil has stable performance.

[0006] A method for preparing a composite copper foil, comprising an amorphous silicon film layer, a flexible base film layer, and a copper film layer, characterized in that the method comprises the following steps: (1) coating the amorphous silicon film layer on one side surface of a base material; (2) coating the flexible base film layer on top of the amorphous silicon film layer; (3) coating the copper film layer on top of the flexible base film layer; and (4) irradiating the amorphous silicon film layer with a laser to peel the amorphous silicon film layer off from the base material.

[0007] Furthermore, after step (1) is completed, silane and hydrogen are introduced to hydrogenate the amorphous silicon film layer.

[0008] Furthermore, the surface temperature of the substrate is 180-300° C. Maintaining a certain temperature of the substrate can better combine the film layer coated on the surface with the substrate.

[0009] Furthermore, the thickness ratio of the amorphous silicon film layer, the flexible base film layer and the copper film layer is 0.5-1.5:0.5-1.5:0.5-1.5.

[0010] Furthermore, the substrate in step (1) is selected from one of quartz glass, ceramics, and nickel-based alloys. The substrate needs to maintain a certain temperature, and a high-temperature resistant material is selected.

[0011] Furthermore, in step (1), the pressure of coating the amorphous silicon film layer is 0-60 Pa and the temperature is 180-300°C.

[0012] Furthermore, the silane concentration is ≥70%. The amorphous silicon film is hydrogenated under high concentration of silane. The amorphous silicon film contains more hydrogen-containing groups and generates hydrogen under laser irradiation.

[0013] Furthermore, the hydrogenation time of the amorphous silicon film is 0 to 10 minutes.

[0014] Furthermore, the coating of the flexible base film layer in step (2) is preferably one of polyimide, polyaramid, and polyamide-imide. The flexible base film layer is made of a high temperature resistant polymer material.

[0015] Furthermore, the coating method in step (2) is a brushing method, a spraying method, or a dipping method.

[0016] Furthermore, the coating method in step (3) is vacuum evaporation, magnetron sputtering, or ion beam sputtering.

[0017] Furthermore, the thickness of the copper film layer in step (3) is 0.1 to 10 μm.

[0018] Furthermore, the energy density of the laser in step (4) is 44 to 60 J / cm2.

[0019] Furthermore, the line width of the laser in step (4) is 170 to 210 μm.

[0020] Furthermore, a composite copper foil is prepared by any of the methods described above.

[0021] Furthermore, the thickness of the composite copper foil is 0.2-20 μm.

[0022] A double-sided composite copper foil comprises the two composite copper foils described in any one of the above items and is formed by gluing the two composite copper foils.

[0023] The composite copper foil prepared by the above method has a small peeling force when peeled from the substrate, and the composite film layer structure will not be damaged during peeling. The film layer is uniform and the composite copper foil has stable performance. The product of the present invention can adjust the thickness of the final composite copper foil by adjusting the thickness of the flexible polymer layer, so as to achieve a thinner composite copper foil that cannot be achieved by the current method. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the structure of a composite copper foil of the present application.

[0025] Figure 2It is a schematic diagram of the interface between the amorphous silicon film layer and the substrate when the composite copper foil of the present application is peeled off from the substrate.

[0026] Figure 3 This is a schematic diagram of the interface structure between an amorphous silicon film layer and a substrate when a composite copper foil is peeled off from a substrate in the present application. DETAILED DESCRIPTION

[0027] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the process equipment or devices not specifically noted in the following embodiments all adopt conventional equipment or devices in the art. In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the presence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combined connection relationship between one or more devices / devices mentioned in the present invention does not exclude the presence of other devices / devices before and after the combination device / device or the insertion of other devices / devices between these explicitly mentioned two devices / devices, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, rather than limiting the order of arrangement of each method step or limiting the scope of the 3 that the present invention can implement. The change or adjustment of its relative relationship, without substantial change in the technical content, should also be regarded as the scope of the present invention that can be implemented.

[0028] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0029] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art in the technical field of the present application. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. It should be noted that, unless otherwise specified, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" include the number, and the meaning of "multiple" in "one or more" is more than two.

[0031] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0032] The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings of the present invention.

[0033] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0034] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art in the technical field of the present application. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. It should be noted that, unless otherwise specified, the term "and / or" used herein includes any and all combinations of one or more related listed items, and "above" and "below" include the number, and the meaning of "multiple" in "one or more" is more than two.

[0036] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0037] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0038] The present invention provides a composite copper foil 1 composed of an amorphous silicon film layer 12, a flexible base film layer 13, and a copper film layer 14. The amorphous silicon film layer 12 is plated on one side of a base material 11. The amorphous silicon film layer 12 is hydrogenated in a high concentration silane environment for a certain period of time. A flexible base film layer 13 is coated on the amorphous silicon film layer 12. The copper film layer 14 is plated on the flexible base film layer. After the coating is completed, the composite copper foil 1 is irradiated with a laser 2 to separate the amorphous silicon film layer 12 from the base material 11. The amorphous silicon film layer 12 is peeled off from the base material 11 to manufacture a composite copper foil 1.

[0039] In the embodiment of the present invention, the amorphous silicon film layer 12 is hydrogenated in a high concentration silane environment, which can increase the hydrogen content of the amorphous silicon film layer. After the coating is completed, after irradiation by the laser 2, a large amount of hydrogen is released from the amorphous silicon film layer 12, and a large number of bubbles 121 are formed at the bonding interface of the amorphous silicon film layer 12 on the substrate 11. Under the action of the laser 2 and the bubbles 121, the amorphous silicon film layer 12 and the substrate 11 can be easily peeled off without damaging the structure of the composite copper foil 1.

[0040] The silane concentration in the present invention refers to the ratio of the silane flow rate to the total gas flow rate (silane + hydrogen) in the gas introduced when hydrogenating the amorphous silicon film layer 12. The silane concentration affects the hydrogen content of the amorphous silicon film layer 12, and ultimately affects the peeling effect of the amorphous silicon film layer 12 and the substrate 11. The higher the hydrogen content of the amorphous silicon film layer 12, the more bubbles are generated under the irradiation of the laser, and the better the peeling effect of the amorphous silicon film layer 12 and the substrate 11.

[0041] In the embodiment, the calculation method of the peeling ratio=the area of ​​the film layer that can be peeled / the total area of ​​the film layer; the calculation method of the tearing ratio=the area of ​​the film layer where the tearing occurs / the total area of ​​the film layer.

[0042] There are many methods for measuring conductivity, such as the three-probe method, the Hall effect method, the extended resistance method, the four-probe method, etc. The four-probe method is a widely used standard method with the advantages of simple equipment, easy operation and high accuracy. The four-probe test technology uses four equally spaced probes to pierce the surface of the semiconductor. A constant current source provides a suitably small current I to the two outer probes, and then measures the voltage V between the two middle probes to calculate the resistivity of the semiconductor. Conductivity is the reciprocal of resistivity.

[0043] When observing bubbles, you can choose a CCD detector (photon detector). For larger bubbles at the micron level, the most direct way to shoot and detect them is through the dynamic image method. The dynamic image method uses a light source to directly illuminate the particles flowing through the detection area, and uses a CCD detector to obtain real-time projections of all particles. It can count the particle size and number of all particles flowing through in real time, and can distinguish micron bubbles from other types of substances through parameters such as the sphericity and aspect ratio of the particles. It can also explore the impact of different factors on micron bubbles through the difference in bubble size and concentration, and evaluate the practical application value of micron bubbles.

[0044] Selection of substrate: Choose quartz glass, ceramics, and nickel-based alloys with smooth surfaces and no obvious defects. These three materials are high-temperature resistant materials, which can prevent the substrate material from melting due to intolerance to high temperatures during laser irradiation.

[0045] Preparation of amorphous silicon film: The preparation methods of amorphous silicon thin films can be divided into two categories based on the preparation principle: physical methods and chemical methods. Commonly used physical methods include electron beam physical vapor deposition and magnetron sputtering; commonly used chemical methods are chemical vapor deposition, mainly including plasma enhanced chemical vapor deposition, radio frequency glow discharge plasma chemical vapor deposition, microwave plasma chemical vapor deposition, etc. The film prepared by the physical method magnetron sputtering has good density, few pinholes, good film adhesion, and high purity. It is easy to automate the process, can be mass-produced, has low energy consumption and production costs, and is one of the main technologies for thin film preparation today. Amorphous silicon film was prepared by magnetron sputtering. The experiment used FJL560 ultra-high vacuum magnetron and ion beam combined sputtering equipment, and the sputtering target was single crystal silicon with a purity of 99.99%. The substrate uses a glass sheet that has been ultrasonically cleaned. The cleaning liquid uses deionized water, acetone and anhydrous ethanol in turn. A DC power supply is used for sputtering. The distance from the substrate to the target surface is 10 cm. The sputtering gas is high-purity (99.99%) argon. Turn on the power, turn on the mechanical pump, and draw a rough vacuum. Then turn on the molecular pump until the working pressure of the system is close to 1.5 Pa. Open the ventilation valve of the argon bottle (99.99% high-purity argon) and pre-flow argon for 20 minutes to remove the adsorbed gas on the pipeline and the vacuum chamber wall. In order to obtain a pure Si film, before depositing the film, first pre-sputter the target for a few minutes to remove impurities on the target. Maintain a power of 60 to 300 W for sputtering. The deposited film is annealed at 300°C and 450°C for 3 minutes respectively; Chemical method Plasma enhanced chemical deposition method Plasma enhanced chemical vapor deposition (PECVD) technology is with the help of PECVD is a new preparation technology that uses glow discharge plasma to make the gaseous substances containing film components react chemically, thereby realizing the growth of thin film materials. Since PECVD technology prepares thin films by gas discharge, it effectively utilizes the reaction characteristics of non-equilibrium plasma and fundamentally changes the energy supply mode of the reaction system. Generally speaking, when using PECVD technology to prepare thin film materials, the growth of thin films mainly includes the following three basic processes: first, in non-equilibrium plasma, electrons react with reaction gases to decompose the reaction gases to form a mixture of ions and active groups; second, various active groups diffuse and transport to the film growth surface and tube wall, and secondary reactions occur between the reactants; finally, various primary reaction and secondary reaction products reaching the growth surface are adsorbed and react with the surface, accompanied by the re-release of gas phase molecules. Specifically, PECVD technology based on glow discharge method can enable the reaction gas to be ionized to form plasma under the excitation of external electromagnetic field.In the plasma of glow discharge, after the electrons are accelerated by the external electric field, their kinetic energy can usually reach about 10eV or even higher, which is enough to destroy the chemical bonds of the reaction gas molecules. Therefore, through the inelastic collision between the high-energy electrons and the reaction gas molecules, the gas molecules will be ionized (ionized) or decomposed to produce neutral atoms and molecular products. The positive ions are accelerated by the ion layer acceleration electric field and collide with the upper electrode. There is also a smaller ion layer electric field near the lower electrode where the substrate is placed, so the substrate is also bombarded by ions to a certain extent. Therefore, the neutral substances produced by the decomposition diffuse to the tube wall and the substrate. These particles and groups (here, chemically active neutral atoms and molecules are all called groups) will undergo ion-molecule reactions and group-molecule reactions during the drift and diffusion process due to the short mean free path. The chemically active substances (mainly groups) that reach the substrate and are adsorbed are very active in chemical properties, and the mutual reactions between them form a film.

[0046] Preparation of flexible substrate film layer: The flexible substrate film layer is selected from one of polyimide, polyarylamide, and polyamide-imide. For example, a polyimide film is prepared by completely dissolving the diamine in an organic solvent, then adding dianhydride and mixing thoroughly, and then injecting the selected glacial acetic acid catalyst for reaction. The entire polymerization process is carried out in a nitrogen and low temperature environment, and then filtered with a 0.1-1.0μm pore size filter element, which is made of PP or PTFE. The filtered polyimide prepolymer is heated for imidization reaction to obtain a polyimide prepolymer with an imidization degree of not less than 80%; wherein the polymerization temperature and time are first stirred at -20--2°C for 2 hours, and then continuously stirred at 25°C for 12 hours; (2) The polyimide film for AMOLED is obtained by casting the polyimide prepolymer; wherein the casting process is to prepare a polyimide film with an imidization degree of not less than 99% under the baking conditions of the preferred multi-gradient temperature and heating and cooling rate, and the preferred multi-gradient temperature heating rate is The cooling process is to dry the wet film with hot air at 80-150°C or on a hot plate for 1 hour, then peel off the film and put it into a high-temperature oven, or put a composite substrate of polyimide film and glass into a high-temperature oven, and pass high-purity nitrogen into the high-temperature oven. After 1 hour, the oxygen content in the oven is not higher than 1000ppm. The temperature gradient is set as follows: heating to 120°C in 30 minutes, maintaining at 120°C for 10 minutes, heating to 150°C in 10 minutes, maintaining at 150°C for 10 minutes, heating to 180°C in 10 minutes, maintaining at 180°C for 10 minutes, heating to 250°C in 23 minutes, maintaining at 250°C for 10 minutes, heating to 450°C in 1 hour and 7 minutes, maintaining at 450°C for 20 minutes, cooling to 180°C in 1 hour and 15 minutes, and cooling to 50°C in 1 hour and 5 minutes; the oxygen concentration in the film baking environment is 0-1000ppm. The preparation of polyaromatic amide and polyamide-imide film layers can also be prepared in this way. The prepared flexible base film layer is coated on the substrate by one or more methods selected from spin coating, hot pressing, electrostatic spraying, plasma spraying, slit coating, anilox coating, micro-concave coating, comma blade coating, screen printing, vapor deposition, vacuum coating, and thermal spraying.

[0047] Preparation of copper film layer: sputtering, electroplating, electron beam evaporation and ion plating are usually used to coat copper film layer. For example, when magnetron sputtering copper film layer is plated, micro-particle magnetron sputtering coating equipment is used. This equipment is based on the ordinary DC magnetron sputtering coating equipment, and an ultrasonic vibration generator is added. During sputtering coating, the micro-particles can maintain good dispersion by adjusting the swing frequency of the sample holder and the vibration power of the ultrasonic wave, and a metal film can be deposited on the surface of the micro-particles by adjusting various sputtering conditions. The target material used for sputtering is a circular Cu target with a purity of 99.99%, a diameter of 10cm and a thickness of 0.5cm. The target material is placed on a target holder connected to a cooling circulating water device, and 1g of silicon carbide powder particles with an average particle size of 60μm are placed in the sample dish on the sample holder. The target-base distance is 17cm. After the vacuum chamber is evacuated, argon gas with a purity of 99.99% is introduced. The gas flow rate is controlled by a mass flow meter, and the sputtering gas pressure is 9x10 -1 Pa, the sputtering power is 50 ~ 400W, the sputtering time and substrate temperature are controlled to obtain copper film layers with different parameters and performances.

[0048] There are many types of lasers, including solid lasers, gas lasers, dye lasers, semiconductor lasers, fiber lasers, and free electron lasers. The laser of the present invention can be a semiconductor laser, and the wavelength is selected to be 650nm. Semiconductor lasers are lasers that use semiconductor materials as working substances. Due to differences in material structure, the specific process of generating lasers of different types is relatively special. Common working substances include gallium arsenide (GaAs), cadmium sulfide (CdS), indium phosphide (InP), zinc sulfide (ZnS), etc. There are three types of excitation methods: electrical injection, electron beam excitation, and optical pumping. Semiconductor laser devices can be divided into several types, such as homojunction, single heterojunction, and double heterojunction. Homojunction lasers and single heterojunction lasers are mostly pulse devices at room temperature, while double heterojunction lasers can achieve continuous operation at room temperature.

[0049] Embodiment 1:

[0050] A preparation method of a composite copper foil and a composite copper foil 1, the preparation method refers to the following steps: adjusting the pressure in the vacuum chamber of plasma chemical vapor deposition to 30Pa and the temperature to 220°C, coating an amorphous silicon film layer 12 on one side surface of a quartz glass 11, after the coating is completed, introducing silane and hydrogen (silane concentration is 90%), hydrogenating for 5 minutes, after the hydrogenation is completed, coating a polyimide (PI) film layer 13 on the top of the amorphous silicon film layer 12, after the coating is completed, magnetron sputtering a copper film layer on the top of the polyimide film layer 13, the film layer thickness is 2μm. After the copper film layer is plated, the amorphous silicon film layer 12 is irradiated with a laser 2 with an energy density of 46 J / cm2, and the line width of the laser 2 is 200 μm. A large number of bubbles 121 appear at the bonding interface between the amorphous silicon film layer 12 and the quartz glass 11. Under the irradiation of the laser 2, the amorphous silicon film layer 12 and the quartz glass 11 are peeled off, and the composite copper foil 1 is peeled off from the quartz glass 11, so as to obtain a composite copper foil 1 with a thickness of 5 μm, a peeling ratio of L1, and a tearing ratio of the amorphous silicon film layer 12 of S1. The composite copper foil 1 is cut into 8 test modules using FIB technology, and the conductivity values ​​E1-1, E1-2, E1-3, E1-4, E1-5, E1-6, E1-7, and E1-8 of each test module are measured respectively.

[0051] Embodiment 2:

[0052] A preparation method of a composite copper foil and a composite copper foil 1, the preparation method refers to the following steps: adjusting the pressure in the vacuum chamber of plasma chemical vapor deposition to 30Pa and the temperature to 220°C, coating an amorphous silicon film layer 12 on one side surface of a quartz glass 11, and after the plating is completed, coating a polyimide (PI) film layer 13 on the top of the amorphous silicon film layer 12, and after the coating is completed, magnetron sputtering a copper film layer on the top of the polyimide film layer 13, the film layer thickness is 2μm. After the copper film layer is plated, the composite copper foil 1 is irradiated with a laser 2 with an energy density of 58 J / cm2 and a line width of 200 μm. A large number of bubbles 121 appear at the interface between the amorphous silicon film layer 12 and the quartz glass 11. Under the irradiation of the laser 2, the amorphous silicon film layer 12 and the quartz glass 11 are peeled off, and the composite copper foil 1 is peeled off from the quartz glass 11, so as to obtain a composite copper foil 1 with a thickness of 5 μm, a peeling ratio of L2, and a tearing ratio of the amorphous silicon film layer 12 of S2. The ultra-thin composite copper foil 1 is cut into 8 test modules using FIB technology, and the conductivity values ​​E2-1, E2-2, E2-3, E2-4, E2-5, E2-6, E2-7, and E2-8 of each test module are measured respectively.

[0053] Embodiment 3:

[0054] A preparation method of a composite copper foil and a composite copper foil 1, the preparation method refers to the following steps: adjusting the pressure in the vacuum chamber of plasma chemical vapor deposition to 45Pa and the temperature to 260°C, coating an amorphous silicon film layer 12 on one side surface of a ceramic 11, after the plating is completed, introducing silane and hydrogen (silane concentration is 80%), hydrogenating for 8 minutes, after the hydrogenation is completed, coating a polyamide (PA) film layer 13 on the top of the amorphous silicon film layer 12, after the coating is completed, magnetron sputtering a copper film layer on the top of the polyimide film layer 13, the film layer thickness is 3μm. After the copper film layer is plated, the amorphous silicon film layer 12 is irradiated with a laser 2 with an energy density of 50 J / cm2, and the line width of the laser 2 is 180 μm. A large number of bubbles 121 appear at the interface between the amorphous silicon film layer 12 and the ceramic 11. Under the irradiation of the laser 2, the amorphous silicon film layer 12 and the ceramic 11 are peeled off, and the composite copper foil 1 is peeled off from the ceramic 11, so as to obtain a composite copper foil 1 with a thickness of 7 μm, a peeling ratio of L3, and a tearing ratio of the amorphous silicon film layer 12 of S3. The ultra-thin composite copper foil 1 is cut into 8 test modules using FIB technology, and the conductivity values ​​E3-1, E3-2, E3-3, E3-4, E3-5, E3-6, E3-7, and E3-8 of each test module are measured respectively.

[0055] Embodiment 4:

[0056] A preparation method of a composite copper foil and a composite copper foil 1, the preparation method refers to the following steps: adjusting the pressure in a vacuum chamber of a plasma chemical vapor deposition to 45 Pa and the temperature to 200° C., coating an amorphous silicon film layer 12 on one side surface of a quartz glass 11, after the coating is completed, introducing silane and hydrogen (silane concentration is 70%), hydrogenating for 7 minutes, coating a polyimide (PI) film layer 13 on the top of the amorphous silicon film layer 12, after the coating is completed, magnetron sputtering a copper film layer on the top of the polyimide film layer 13, the film layer thickness is 0.5 μm. After the copper film layer is plated, the composite copper foil 1 is irradiated with a laser 2 with an energy density of 50 J / cm2, and the line width of the laser 2 is 178 μm. A large number of bubbles 121 appear at the bonding interface between the amorphous silicon film layer 12 and the quartz glass 11. Under the irradiation of the laser 2, the amorphous silicon film layer 12 and the quartz glass 11 are peeled off, and the composite copper foil 1 is peeled off from the quartz glass 11, so as to obtain a composite copper foil 1 with a thickness of 1.2 μm, a peeling ratio of L4, and a tearing ratio of the amorphous silicon film layer 12 of S4. The ultra-thin composite copper foil 1 is cut into 8 test modules using FIB technology, and the conductivity values ​​of each test module are measured respectively, E4-1, E4-2, E4-3, E4-4, E4-5, E4-6, E4-7, and E4-8.

[0057] Embodiment 5:

[0058] Take two sheets of composite copper foil prepared in Examples 1 and 5. Select a precursor such as polyurethane-based, acrylate-based, or butyl rubber-based. Apply glue to the back of the first composite copper foil and the copper-free side of the second composite copper foil, and wait for drying.

[0059] After drying, the first composite copper foil and the second composite copper foil are aligned and stacked, and heat-pressed and bonded under nitrogen protection.

[0060] In this embodiment, the first composite copper foil is 5 μm, and the second composite copper foil is 1.2 μm. After hot pressing and bonding, a double-sided composite copper foil is formed. The thickness of the double-sided composite copper foil is 6.5 μm.

[0061] The method of the present invention can flexibly obtain double-sided composite copper foils of different thicknesses, which can be used in any occasion as needed.

[0062] Comparative Example 1:

[0063] Comparative Example 1 Compared with Example 1, other operating conditions remain unchanged. When the amorphous silicon film layer 12 is hydrogenated, the silane concentration is 10%, and a composite copper foil 1 is prepared with a thickness of 5 μm, a peeling ratio of L5, and a tearing ratio of the amorphous silicon film layer 12 of S5. The ultra-thin composite copper foil 1 is cut into 8 test modules using FIB technology, and the conductivity values ​​E5-1, E5-2, E5-3, E5-4, E5-5, E5-6, E5-7, and E5-8 of each test module are measured respectively.

[0064] Comparative Example 2:

[0065] Comparative Example 2 Compared with Example 2, other operating conditions remain unchanged, and the amorphous silicon film layer 12 is not plated, and a composite copper foil 1 is prepared, with a thickness of 5 μm, a peeling ratio of L6, and a tearing ratio of the amorphous silicon film layer 12 of S6. The ultra-thin composite copper foil 1 is cut into 8 test modules using FIB technology, and the conductivity values ​​E6-1, E6-2, E6-3, E6-4, E6-5, E6-6, E6-7, and E6-8 of each test module are measured respectively.

[0066] After measurement and calculation, the values ​​of the peeling ratio and tearing ratio of the embodiments and comparative examples are shown in the following table:

[0067] Table 1 Peel ratio and tear ratio

[0068] Serial number Stripping ratio (%) Tear ratio (%) Example 1 100 0 Example 2 100 0 Example 3 100 0 Example 4 100 0 Comparative Example 1 95 3 Comparative Example 2 70 23

[0069] Table 2 Conductivity value table

[0070]

[0071]

[0072] The above is only a specific implementation of the present application. Under the above teachings of the present application, those skilled in the art can make other improvements or modifications based on the above embodiments. Those skilled in the art should understand that the above specific description is only to better explain the purpose of the present application, and the protection scope of the present application shall be based on the protection scope of the claims.

[0073] In addition, those skilled in the art will appreciate that, although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the claims below, any one of the claimed embodiments may be used in any combination.

Claims

1. A method for preparing a composite copper foil, the composite copper foil comprising an amorphous silicon film layer, a flexible substrate film layer, and a copper film layer. It is characterized in that The following steps are involved: (1) coating the amorphous silicon film layer on one side surface of the substrate. After step (1), introducing silane and hydrogen to hydrogenate the amorphous silicon film layer, wherein the silane concentration is 90%; (2) coating the flexible base film layer on the amorphous silicon film layer; (3) plating a copper film layer on the flexible base film layer; (4) irradiating the amorphous silicon film layer with laser to peel the amorphous silicon film layer off from the substrate; the energy density of the laser in step (4) is 44 to 60 J / cm2; the line width of the laser in step (4) is 170 to 210 μm; The thickness ratio of the amorphous silicon film layer, the flexible base film layer and the copper film layer is 0.5-1.5:0.5-1.5:0.5-1.

5.

2. The method for preparing a composite copper foil according to claim 1, It is characterized in that The surface temperature of the substrate is 180-300°C.

3. The method for preparing a composite copper foil according to claim 1, It is characterized in that The substrate in step (1) is selected from one of quartz glass, ceramics, and nickel-based alloy.

4. The method for preparing a composite copper foil according to claim 1, It is characterized in that The pressure of coating the amorphous silicon film layer in step (1) is 0-60 Pa and the temperature is 180-300°C.

5. The method for preparing a composite copper foil according to claim 1, It is characterized in that The hydrogenation time of the amorphous silicon film layer is 0 to 10 minutes.

6. The method for preparing a composite copper foil according to claim 1, It is characterized in that The coating of the flexible base film layer in step (2) is one of polyimide, polyaramid and polyamide-imide.

7. The method for preparing a composite copper foil according to claim 1, It is characterized in that The coating method in step (2) is brushing, spraying or dipping.

8. The method for preparing a composite copper foil according to claim 1, It is characterized in that The plating method in step (3) is vacuum evaporation, magnetron sputtering, or ion beam sputtering.

9. The method for preparing a composite copper foil according to claim 1, It is characterized in that The thickness of the copper film layer in step (3) is 0.1 to 10 μm.

10. A composite copper foil prepared according to the method according to any one of claims 1 to 9.

11. A composite copper foil according to claim 10, It is characterized in that The thickness is 0.2~20μm.

12. The composite copper foil according to claim 10, It is characterized in that The conductivity is 0.8×10 4 ~5×10 5 S / cm.

13. A double-sided composite copper foil, Features: The double-sided composite copper foil comprises two sheets of composite copper foil as described in any one of claims 10 to 12, and is formed by gluing the two sheets of composite copper foil.