A porous polymer millimeter ball and preparation method thereof
By adding linear polymers during the polymerization process and post-extraction cross-linking process, porous polymer millimeter spheres with high specific surface area were prepared, which solved the problem of poor adsorption effect of porous polymer materials in large industrial equipment in the existing technology. It solves the best problem and achieves efficient removal of organic waste gas.
Patent Information
- Application Number
- CN202311019657.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-08-14
AI Technical Summary
Existing porous polymer materials exist in the form of nano-sized powders, which are difficult to apply to organic waste gas treatment in large-scale industrial equipment. Moreover, the adsorption effect of large-sized zeolite molecular sieves on organic waste gas is not ideal, making it difficult to effectively remove organic waste gas in industrial production. pollute.
Cross-linked polystyrene millimeter-scale porous microspheres are synthesized by adding linear polymer as a template during the polymerization process. The linear polymer is used to adjust the viscosity of the polymerized monomer and act as a porogen. Combined with the later extraction process and Cross-linking solvent weaving method forms porous polymer millimeter spheres with high specific surface area, improving its small molecule adsorption capacity.
It has achieved strong adsorption capacity for small molecules and increased the pore volume and specific surface area of millimeter-sized spherical polymer particles. It is suitable for organic waste gas treatment in large industrial equipment and improves the adsorption efficiency.
Smart Images

Figure CN116903916B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer functional materials, and in particular relates to a porous polymer millimeter ball and a preparation method thereof. Background Art
[0002] The emission of organic waste gas generated in industrial production into the air will pollute the atmosphere and cause damage to the health of surrounding people or animals, such as carcinogenicity and teratogenicity. However, in large-scale industrial production equipment, porous polymer adsorption materials with the best adsorption efficiency for organic waste gas generally exist in the form of nano-sized powders, which requires the design of adsorption beds for collection and regeneration during use. Large-sized zeolite molecular sieves generally have good hydrophilicity and have poor adsorption effects on organic waste gas. Therefore, millimeter-sized spherical polymer adsorption materials have high practical value in the process of organic waste gas treatment.
[0003] Conventional cross-linked polystyrene white balls synthesized by suspension polymerization can reach millimeter-scale spherical particles, but they are almost pore-free inside and have a small specific surface area. Porous polymer materials with high specific surface areas are generally in the micron to nanometer scale and are not suitable for large-scale industrial equipment. Summary of the invention
[0004] In order to solve the above problems existing in the prior art, the present invention provides a porous polymer millimeter ball and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0005] A method for preparing porous polymer millimeter balls comprises the following steps:
[0006] Step 1: preheat the aqueous phase containing the surfactant to 70-90°C;
[0007] Step 2: Stir polystyrene, styrene, divinylbenzene and initiator until homogeneous, add preheated aqueous phase containing surfactant dropwise under mechanical stirring, and perform polymerization reaction for 3-5 hours;
[0008] Step 3: filtering the product obtained in step 2, washing with water, extracting with a solvent, and drying to obtain a spherical polymer;
[0009] Step 4: Swell the spherical polymer obtained in step 3 in dichloroethane, add dimethoxymethane and Lewis acid catalyst, react at room temperature, filter the obtained product, soak it in hydrochloric acid, filter it again, wash it with water and dichloroethane in turn, and dry it to obtain porous polymer millimeter balls.
[0010] Furthermore, the preparation method of the above polystyrene is: add styrene, ammonium persulfate and sodium dodecyl sulfate into deionized water, perform polymerization reaction at 60-80°C for 3-5 h, dry at 50-60°C and grind.
[0011] Furthermore, in the above step 1, the surfactant is selected from at least one of polyvinyl alcohol, sodium lauryl sulfate and hexadecyltrimethylammonium bromide, and the concentration of the aqueous phase containing the surfactant is 0.1% to 1.5%.
[0012] Furthermore, in the above step 2, the volume ratio of styrene to divinylbenzene is 3:1~39:1, the ratio of the mass of polystyrene to the sum of the volumes of styrene and divinylbenzene is 1g:4mL~3g:4mL, and the ratio of the sum of the volumes of styrene and divinylbenzene to the volume of the aqueous phase is 4%.
[0013] Furthermore, in the above step 2, the initiator is selected from azobisisobutyronitrile or benzoyl peroxide, and the mechanical stirring speed in the step 2 is 200 rpm~400 rpm.
[0014] Furthermore, the solvent used in the above step three is selected from dichloromethane or tetrahydrofuran, and the drying temperature is 50-55°C.
[0015] Furthermore, in the above step 4, the Lewis acid catalyst is selected from anhydrous aluminum chloride or anhydrous ferric chloride.
[0016] Furthermore, in the above step 4, the reaction time is 18-24 hours, the soaking time is 1-3 hours, and the drying temperature is 50-55°C.
[0017] A porous polymer millimeter ball is prepared by adopting the above-mentioned preparation method of the porous polymer millimeter ball.
[0018] Furthermore, the average particle size of the porous polymer millimeter spheres is 2 mm.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention synthesizes cross-linked polystyrene millimeter-scale porous microspheres by adding a linear high molecular polymer as a template during the polymerization process. The linear high molecular polymer not only adjusts the viscosity of the polymerization monomer, which is beneficial to the formation of stable millimeter-scale spherical particles, but also acts as a porogen to form pores through a subsequent extraction process, thereby increasing the pore volume of the millimeter-scale spherical polymer particles. Finally, a post-cross-linking solvent weaving method is used to further increase the specific surface area of the spherical polymer particles and increase the overall microporous adsorption capacity of the particles, thereby obtaining a strong adsorption capacity for small molecules. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1It is a scanning electron microscope image of the cross section of the unextracted product of Example 1.
[0022] Figure 2 It is a scanning electron microscope image of the cross section of the product after extraction in Example 1.
[0023] Figure 3 It is the infrared spectra of the product obtained after extraction and the product obtained after cross-linking in Example 1.
[0024] Figure 4 It is the nitrogen isotherm adsorption line of the product obtained before and after extraction and the product obtained after cross-linking in Example 1.
[0025] Figure 5 This is an optical photograph of the porous polymer millimeter sphere of Example 1. Implementation
[0026] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.
[0027] The present invention provides a method for preparing porous polymer millimeter balls, which comprises the following steps:
[0028] Step 1: preheating the aqueous phase containing a surfactant to 70-90° C., wherein the surfactant is selected from at least one of polyvinyl alcohol, sodium lauryl sulfate, and hexadecyltrimethylammonium bromide, and the concentration of the aqueous phase containing the surfactant is 0.1%-1.5%.
[0029] Step 2: Stir polystyrene, styrene, divinylbenzene and initiator until homogeneous, add preheated aqueous phase containing surfactant dropwise under mechanical stirring, and carry out polymerization reaction for 3 to 5 hours; wherein, the volume ratio of styrene to divinylbenzene is 3:1 to 39:1, the ratio of the mass of polystyrene to the sum of the volumes of styrene and divinylbenzene is 1g:4mL to 3g:4mL, and the ratio of the sum of the volumes of styrene and divinylbenzene to the volume of the aqueous phase is 4%; the initiator is selected from azobisisobutyronitrile or benzoyl peroxide, and the mechanical stirring speed is 200 rpm to 400 rpm.
[0030] Step 3: The product obtained in step 2 is filtered, washed with water, extracted with a solvent, and dried to obtain a spherical polymer. The solvent used is selected from dichloromethane or tetrahydrofuran, and the drying temperature is 50-55°C. After extraction, the specific surface area can be increased to 5-50 m 2 / g.
[0031] Step 4: Swell the spherical polymer obtained in step 3 in dichloroethane, add dimethoxymethane and Lewis acid catalyst, react at room temperature, filter the obtained product, soak it in hydrochloric acid, filter it again, wash it with water and dichloroethane in sequence, and dry it to obtain porous polymer millimeter balls; wherein the Lewis acid catalyst is selected from anhydrous aluminum chloride or anhydrous ferric chloride, the reaction time is 18-24h, the soaking time is 1-3h, and the drying temperature is 50-55°C. After post-crosslinking, the specific surface area can be increased to 80-120 m 2 / g.
[0032] The preparation method of polystyrene of the present invention comprises the following steps: adding styrene, ammonium persulfate and sodium dodecyl sulfate into deionized water, polymerizing at 60-80° C. for 3-5 h, drying at 50-60° C. and then grinding.
[0033] The present invention also provides a porous polymer millimeter ball, which is prepared by the porous polymer millimeter ball preparation method of the present invention. The average particle size of the porous polymer millimeter ball is 2 mm. Embodiment 1:
[0034] Preheat 100 mL of 0.1% mass fraction sodium dodecyl sulfate solution to 80°C, dissolve 1.5 g of polystyrene and 0.05 g of azobisisobutyronitrile in 3 mL of styrene and 1 mL of divinylbenzene and stir until homogeneous and transparent, add the above solution dropwise into the preheated sodium dodecyl sulfate solution under mechanical stirring at 250 rpm, and react at 80°C for 4 h. After the reaction is completed, filter the product, wash with water, use solvent tetrahydrofuran to fully extract the product in a Soxhlet extraction device for 24 h, and dry at 55°C; take 0.2 g of spherical polymer and load it with 25 mL of dichloroethane, add 0.3 g of anhydrous aluminum chloride and 0.1 mL of dimethylformal for post-crosslinking treatment, react at room temperature for 24 h, filter, soak in hydrochloric acid for 1 h, filter again, wash with water and dichloroethane in turn, and dry at 55°C to obtain porous polymer millimeter spheres.
[0035] The preparation method of polystyrene in this embodiment is as follows: 25 mL of styrene, 1 g of ammonium persulfate, and 1.5 g of sodium dodecyl sulfate are added to 500 mL of deionized water, polymerized at 70° C. for 4 h, dried at 60° C., and then ground.
[0036] The scanning electron microscope image of the cross section of the unextracted product in this example is as follows Figure 1 ,from Figure 1 It can be seen that the unextracted product has a dense structure. The scanning electron microscope image of the cross section of the product after extraction in this embodiment is as follows Figure 2 ,from Figure 2It can be seen that the linear polymer leaves obvious pores after extraction, and the specific surface area increases to 50 m 2 / g. The infrared spectra of the product after extraction and the product obtained by post-crosslinking are shown in Figure 3 The nitrogen isotherm adsorption curves of the products before and after extraction and the products after cross-linking are shown in Figure 4 As shown, from Figure 4 It can be seen that the specific surface area is increased after extraction and cross-linking. In this embodiment, the specific surface area can be increased to 120 m after post-cross-linking. 2 / g. Figure 5 This is an optical photograph of the porous polymer millimeter sphere of this example. Embodiment 2:
[0037] Preheat 100 mL of 0.1% mass fraction polyvinyl alcohol solution to 70°C, dissolve 1.5 g polystyrene and 0.1 g benzoyl peroxide in 6 mL styrene and 1 mL divinylbenzene, stir until homogeneous and transparent, add the above solution dropwise to the preheated polyvinyl alcohol solution under mechanical stirring at 200 rpm, and react at 70°C for 5 h. After the reaction is completed, filter the product, wash with water, use solvent tetrahydrofuran to fully extract the product in a Soxhlet extraction device for 24 h, and dry it at 50°C; take 0.2 g of spherical polymer and load it into 25 mL tetrahydrofuran, add 0.3 g anhydrous ferric chloride and 0.1 mL dimethylformal for post-crosslinking treatment, react at room temperature for 24 h, filter it, soak it in hydrochloric acid for 3 h, filter it again, wash it with water and dichloroethane in turn, and dry it at 53°C to obtain porous polymer millimeter spheres.
[0038] After extraction, the specific surface area of this embodiment can be increased to 30 m 2 / g. After post-crosslinking, the specific surface area can be increased to 105m 2 / g.
[0039] The preparation method of polystyrene in this embodiment is as follows: 25 mL of styrene, 1 g of ammonium persulfate, and 1.5 g of sodium dodecyl sulfate are added to 500 mL of deionized water, polymerized at 70° C. for 4 h, dried at 60° C., and then ground. Embodiment 3:
[0040] Preheat 100 mL of 0.1% mass fraction hexadecyltrimethylammonium bromide solution to 90°C, dissolve 1.5 g of polystyrene and 0.1 g of azobisisobutyronitrile in 6 mL of styrene and 1 mL of divinylbenzene and stir until homogeneous and transparent, add the above solution dropwise to the preheated hexadecyltrimethylammonium bromide solution under mechanical stirring at 400 rpm, and react at 90°C for 3 hours. After the reaction is completed, filter the product, wash with water, use solvent dichloromethane to fully extract the product in a Soxhlet extraction device for 24 hours, and dry it at 55°C; take 0.2 g of spherical polymer and load it into 25 mL of tetrahydrofuran, add 0.3 g of anhydrous ferric chloride and 0.1 mL of dimethylformal for post-crosslinking treatment, react at room temperature for 18 hours, filter it, soak it in hydrochloric acid for 2 hours, filter it again, wash it with water and dichloroethane in turn, and dry it at 50°C to obtain porous polymer millimeter balls.
[0041] After extraction, the specific surface area of this embodiment can be increased to 25 m 2 / g. After post-crosslinking, the specific surface area can be increased to 110m 2 / g.
[0042] The preparation method of polystyrene in this embodiment is as follows: 25 mL of styrene, 1 g of ammonium persulfate, and 1.5 g of sodium dodecyl sulfate are added to 500 mL of deionized water, polymerized at 70° C. for 4 h, dried at 60° C., and then ground. Embodiment 4:
[0043] Preheat 100 mL of 0.1% mass fraction sodium dodecyl sulfate solution to 80°C, dissolve 1.5 g of polystyrene and 0.05 g of azobisisobutyronitrile in 3 mL of styrene and 1 mL of divinylbenzene and stir until homogeneous and transparent, add the above solution dropwise into the preheated sodium dodecyl sulfate solution under mechanical stirring at 250 rpm, and react at 80°C for 4 h. After the reaction is completed, filter the product, wash with water, use solvent dichloromethane to fully extract the product for 18 h in a Soxhlet extraction device, and dry it at 55°C; take 0.2 g of spherical polymer and load it into 30 mL of dichloroethane, add 0.5 g of anhydrous ferric chloride and 0.1 mL of dimethylformal for post-crosslinking treatment, react at room temperature for 24 h, filter it, soak it in hydrochloric acid for 1 h, filter it again, wash it with water and dichloroethane in turn, and dry it at 55°C to obtain porous polymer millimeter spheres.
[0044] After extraction, the specific surface area of this embodiment can be increased to 20 m 2 / g. After post-crosslinking, the specific surface area can be increased to 115m 2 / g.
[0045] The preparation method of polystyrene in this embodiment is as follows: 25 mL of styrene, 1 g of ammonium persulfate, and 1.5 g of sodium dodecyl sulfate are added to 500 mL of deionized water, polymerized at 70° C. for 4 h, dried at 60° C., and then ground.
[0046] The present invention synthesizes cross-linked polystyrene millimeter-scale porous microspheres by adding a linear high molecular polymer as a template during the polymerization process. The linear high molecular polymer not only adjusts the viscosity of the polymerization monomer, which is beneficial to the formation of stable millimeter-scale spherical particles, but also acts as a porogen to form pores through a subsequent extraction process, thereby increasing the pore volume of the millimeter-scale spherical polymer particles. Finally, a post-cross-linking solvent weaving method is used to further increase the specific surface area of the spherical polymer particles and increase the overall microporous adsorption capacity of the particles, thereby obtaining a strong adsorption capacity for small molecules.
[0047] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing porous polymer millimeter balls, characterized in that: The steps include: Step 1: preheat the aqueous phase containing the surfactant to 70-90°C; Step 2: Stir polystyrene, styrene, divinylbenzene and initiator until homogeneous, add preheated aqueous phase containing surfactant dropwise under mechanical stirring, and perform polymerization reaction for 3 to 5 hours; Step 3: filtering the product obtained in step 2, washing with water, extracting with a solvent, and drying to obtain a spherical polymer; Step 4: Swell the spherical polymer obtained in step 3 in dichloroethane, add dimethoxymethane and Lewis acid catalyst, react at room temperature, filter the obtained product, soak it in hydrochloric acid, filter it again, wash it with water and dichloroethane in turn, and dry it to obtain porous polymer millimeter balls, wherein the average particle size of the porous polymer millimeter balls is 2 mm.
2. The method for preparing porous polymer millimeter balls according to claim 1, characterized in that: The preparation method of polystyrene in step 2 is: adding styrene, ammonium persulfate and sodium dodecyl sulfate into deionized water, polymerizing at 60-80° C. for 3-5 hours, drying at 50-60° C. and then grinding.
3. The method for preparing porous polymer millimeter balls according to claim 1, characterized in that: In the step 1, the surfactant is selected from at least one of polyvinyl alcohol, sodium lauryl sulfate and hexadecyltrimethylammonium bromide, and the concentration of the aqueous phase containing the surfactant is 0.1% to 1.5%.
4. The method for preparing porous polymer millimeter balls according to claim 1, characterized in that: In the step 2, the volume ratio of styrene to divinylbenzene is 3:1-39:1, the ratio of the mass of polystyrene to the sum of the volumes of styrene and divinylbenzene is 1g:4mL-3g:4mL, and the ratio of the sum of the volumes of styrene and divinylbenzene to the volume of the water phase is 4%.
5. The method for preparing porous polymer millimeter balls according to claim 1, characterized in that: In the step 2, the initiator is selected from azobisisobutyronitrile or benzoyl peroxide, and the mechanical stirring speed in the step 2 is 200 rpm to 400 rpm.
6. The method for preparing porous polymer millimeter balls according to claim 1, characterized in that: The solvent used in step three is selected from dichloromethane or tetrahydrofuran, and the drying temperature is 50-55°C.
7. The method for preparing porous polymer millimeter balls according to claim 1, characterized in that: In the step 4, the Lewis acid catalyst is selected from anhydrous aluminum chloride or anhydrous ferric chloride.
8. The method for preparing porous polymer millimeter balls according to claim 1, characterized in that: In the step 4, the reaction time is 18 to 24 hours, the soaking time is 1 to 3 hours, and the drying temperature is 50 to 55°C.
9. A porous polymer millimeter ball, characterized in that: The porous polymer millimeter ball is prepared by the preparation method of any one of claims 1 to 8.