A fire retardant coating for metal casing of power battery and preparation method thereof

By preparing a fire-retardant coating containing water-based polyurethane emulsion, aluminum nitride, aluminum phosphate, and silica, the problems of thickness and durability of existing coatings were solved, achieving high-efficiency fire resistance and thermal conductivity of thin coatings, and protecting the safety of the power battery casing.

CN116904097BActive Publication Date: 2024-11-01SUZHOU HONGJU METAL PROD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310875941.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-17
Publication Date
2024-11-01
Estimated Expiration
2043-07-17

AI Technical Summary

Technical Problem

Existing fire-retardant coatings require a thick coating to produce the desired fire-retardant effect, and the coating is prone to cracking and peeling, and its poor thermal conductivity affects the fire-retardant effect.

Method used

The aerogel is made by stirring, freeze-drying and pressing water-based polyurethane emulsion, aluminum nitride, aluminum phosphate and fumed silica as the main components. It is then ground to a specific particle size, water is added to make a coating, and it is applied to the metal shell of the power battery.

Benefits of technology

It achieves excellent fire resistance under a thin coating, the coating is not easy to crack or peel off, it can conduct heat quickly, and protect the power battery shell to keep the temperature within a safe range at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116904097B_ABST
    Figure CN116904097B_ABST
Patent Text Reader

Abstract

The invention discloses a fire retardant coating for a metal shell of a power battery and a preparation method thereof. First, 15-25 parts by mass of aluminum nitride, 15-25 parts by mass of aluminum phosphate and 15-25 parts by mass of white carbon are sieved through a 3000-7000 mesh sieve; then 25-37.5 parts by mass of an aqueous polyurethane emulsion are stirred and mixed with the sieved aluminum nitride, aluminum phosphate and white carbon; the mixture is placed in a freeze dryer, freeze-dried, and made into an aerogel; then the aerogel is pressed at 20-30 degrees Celsius, pressed at a pressure of 1-10 MPa, and then the pressed aerogel is ground to a particle size within the range of 1-10 microns; water is added to the ground aerogel, wherein the mass of all solid raw materials accounts for 25-40% of the mass of water, and stirred and mixed to obtain a coating. When the coating prepared by the present invention is coated at a thickness of 300-500 microns, the temperature of the coated metal inner layer can be kept within 100 degrees Celsius within 60 seconds under the burning of a 1300-1400 degrees Celsius flame, and is very suitable for fire protection of power battery casings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coating preparation, and in particular to a fire retardant coating for a metal casing of a power battery and a preparation method thereof. Background Art

[0002] Fire retardant coatings have a wide range of applications in many fields, such as construction, transportation, electricity, aerospace, etc. Fire retardant coatings are designed to reduce the flammability of the coated material, slow the spread of fire, and protect the substrate from high temperature damage. Common types of fire retardant coatings include organic fire retardant coatings (such as water-based, solvent-based, etc.), inorganic fire retardant coatings (such as cement-based, silicate-based, etc.) and aerogel fire retardant coatings. However, the fire retardant coatings currently on the market still have some problems in practical applications, such as the need for thicker coatings to produce ideal fire protection effects, and the coatings are prone to cracking, falling off and other problems. In addition, poor thermal conductivity may cause the heat in the fire source area to be unable to be quickly transferred to other areas, thereby affecting the fire protection effect.

[0003] Therefore, developing a new type of fire-retardant coating with excellent fire-retardant properties and a thinner coating can not only improve the fire-retardant effect, but also reduce the weight of the coating and reduce problems such as coating cracking and falling off, which is of great practical significance. Summary of the invention

[0004] The purpose of the present invention is to provide a fire retardant coating for a metal casing of a power battery.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned fire retardant coating for the metal casing of a power battery.

[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: a fire retardant coating for the metal casing of a power battery, mainly composed of the following components in parts by mass: 25-37.5 parts by mass of an aqueous polyurethane emulsion, 15-25 parts by mass of aluminum nitride, 15-25 parts by mass of aluminum phosphate, and 15-25 parts by mass of white carbon black.

[0007] Another aspect of the present invention is to provide a method for preparing the fire retardant coating for the metal casing of a power battery, comprising the following steps:

[0008] Step 1: sieve aluminum nitride, aluminum phosphate and white carbon black through a 3000-7000 mesh sieve; then stir and mix the waterborne polyurethane emulsion with the sieved aluminum nitride, aluminum phosphate and white carbon black;

[0009] Step 2: placing the mixture into a freeze dryer, freeze drying, and forming an aerogel; then pressing the aerogel at 20-30 degrees Celsius and using a pressure of 1-10 MPa, and then grinding the pressed aerogel to a particle size in the range of 1-10 microns;

[0010] Step 3: adding water to the ground aerogel, wherein the mass of all solid raw materials accounts for 25-40% of the mass of water, stirring and mixing to obtain a coating.

[0011] Preferably, in step 1, the stirring speed is 200-300 rpm, and the stirring time is 20-30 minutes.

[0012] Preferably, in step 1, the temperature during the freeze-drying process is set at -50 to -40 degrees Celsius, and the freeze-drying time is 24-48 hours.

[0013] Preferably, in step three, the stirring speed is 200-300 rpm, and the stirring time is 20-30 minutes.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] 1. The present invention provides a fire retardant coating for a power battery metal casing and a preparation method thereof. When the coating is coated at a thickness of 300-500 microns, the temperature of the coated metal inner layer can be kept within 100 degrees Celsius within 60 seconds under the burning of a 1300-1400 degrees Celsius flame, which is very suitable for fire protection of power battery casings. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the temperature rise curve of the inner and outer surfaces of the burning test after the coating of Example 1 is applied to the metal. DETAILED DESCRIPTION

[0017] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0018] The mass fraction of the aqueous polyurethane emulsion used in the following examples is 30% to 40%, and commercially available aluminum nitride with a purity of 99% to 99.9%, commercially available aluminum phosphate with a purity of 99% to 99.9%, and commercially available white carbon black with a purity of 99% to 99.9% are used.

[0019] Example 1

[0020] The main raw materials of the fire retardant coating of this embodiment are: 25 parts by mass of waterborne polyurethane emulsion, 25 parts by mass of aluminum nitride, 15 parts by mass of aluminum phosphate, and 15 parts by mass of white carbon black. The preparation method comprises the following steps:

[0021] 1. First, pass aluminum nitride, aluminum phosphate and white carbon black through a 7000 mesh sieve;

[0022] 2. Stir and mix the aqueous polyurethane emulsion with the sieved aluminum nitride, aluminum phosphate and white carbon black at a stirring speed of 300 rpm for 20 minutes;

[0023] 3. Place the mixture in a freeze dryer, set the temperature to -40 degrees Celsius during the freeze drying process, and freeze dry for 48 hours to produce aerogel;

[0024] 4. Press the aerogel at 20 degrees Celsius using a pressure of 10 MPa;

[0025] 5. Grind the pressed aerogel to a particle size of 1 micron;

[0026] 6. Add water, wherein the mass of all solid raw materials accounts for 40% of the mass of water, stir and mix at a stirring speed of 300 rpm for 20 minutes to prepare a coating.

[0027] Figure 1 This is the temperature rise curve of the inner and outer surfaces of the burning test after the coating of Example 1 is applied to the metal. The coating thickness is 300 microns. When the burning surface temperature reaches 1400 degrees Celsius, the maximum temperature of the inner surface is 97.11 degrees Celsius, and the fireproof effect is obvious.

[0028] Example 2

[0029] The main raw materials of the fire retardant coating of this embodiment are: 37.5 parts by mass of waterborne polyurethane emulsion, 15 parts by mass of aluminum nitride, 25 parts by mass of aluminum phosphate, and 15 parts by mass of white carbon black. The preparation method comprises the following steps:

[0030] 1. First, pass aluminum nitride, aluminum phosphate and white carbon black through a 3000 mesh sieve;

[0031] 2. Stir and mix the aqueous polyurethane emulsion with the sieved aluminum nitride, aluminum phosphate and white carbon black at a stirring speed of 200 rpm for 30 minutes;

[0032] 3. Place the mixture in a freeze dryer, set the temperature to -50 degrees Celsius during the freeze drying process, and freeze dry for 24 hours to produce aerogel;

[0033] 4. Press the aerogel at 30 degrees Celsius using a pressure of 1 MPa;

[0034] 5. Grind the pressed aerogel to a particle size of 10 microns;

[0035] 6. Add water, wherein the mass of all solid raw materials accounts for 25% of the mass of water, stir and mix at a stirring speed of 200 rpm for 30 minutes to prepare a coating.

[0036] Example 3

[0037] The main raw materials of the fire retardant coating of this embodiment are: 31.25 parts by mass of waterborne polyurethane emulsion, 15 parts by mass of aluminum nitride, 25 parts by mass of aluminum phosphate, and 20 parts by mass of white carbon black. The preparation method comprises the following steps:

[0038] 1. First, pass aluminum nitride, aluminum phosphate and white carbon black through a 5000 mesh sieve;

[0039] 2. Stir and mix the aqueous polyurethane emulsion with the sieved aluminum nitride, aluminum phosphate and white carbon black at a stirring speed of 250 rpm for 25 minutes;

[0040] 3. Place the mixture in a freeze dryer, set the temperature to -45 degrees Celsius during the freeze drying process, and freeze dry for 36 hours to produce aerogel;

[0041] 4. Press the aerogel at 25 degrees Celsius using a pressure of 5 MPa;

[0042] 5. Grind the pressed aerogel to a particle size of 5 microns;

[0043] 6. Add water, wherein the mass of all solid raw materials accounts for 35% of the mass of water, stir and mix at a stirring speed of 250 rpm for 25 minutes to prepare a coating.

[0044] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modification, equivalent substitution and improvement made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A fire retardant coating for a metal casing of a power battery, characterized in that: The invention is mainly made of the following components in parts by weight: 25-37.5 parts by weight of aqueous polyurethane emulsion, 15-25 parts by weight of aluminum nitride, 15-25 parts by weight of aluminum phosphate, and 15-25 parts by weight of white carbon black; Prepared by the following steps: Step 1: sieve aluminum nitride, aluminum phosphate and white carbon black through a 3000-7000 mesh sieve; then stir and mix the waterborne polyurethane emulsion with the sieved aluminum nitride, aluminum phosphate and white carbon black; Step 2: placing the mixture into a freeze dryer, freeze drying, and forming an aerogel; then pressing the aerogel at 20-30 degrees Celsius and using a pressure of 1-10 MPa, and then grinding the pressed aerogel to a particle size in the range of 1-10 microns; Step 3, adding water to the ground aerogel, wherein the mass of all solid raw materials accounts for 25-40% of the mass of water, stirring and mixing to obtain a coating.

2. The fire retardant coating for the metal casing of a power battery according to claim 1, characterized in that: In step 1, the stirring speed is 200-300 rpm, and the stirring time is 20-30 minutes.

3. The fire retardant coating for the metal casing of a power battery according to claim 1, characterized in that: In step 2, the temperature during the freeze-drying process is set at -50 to -40 degrees Celsius, and the freeze-drying time is 24-48 hours.

4. The fire retardant coating for a metal casing of a power battery according to claim 1, characterized in that: In step 3, the stirring speed is 200-300 rpm, and the stirring time is 20-30 minutes.