A nano titanium dioxide-zinc oxide composite material

Through the combination of nano-titanium dioxide-zinc oxide composite materials and thiol-modified concave and concave rock stones, the existing photocatalyst recovery problems and low adsorption rate are solved, efficient degradation and adsorption of methylene blue are achieved, and the treatment of organic dye wastewater is significantly improved. effect.

CN116943631BActive Publication Date: 2024-11-15GUIZHOU LEICHENG ENVIRONMENTAL PROTECTION NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311160088.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-11
Publication Date
2024-11-15
Estimated Expiration
2043-09-11

AI Technical Summary

Technical Problem

The existing photocatalysts have problems with recycling difficulties and low adsorption rate when treating organic dye wastewater, and cannot effectively degrade methylene blue.

Method used

Using nanotitanium dioxide-zinc oxide composite material, nanotitanium dioxide is prepared by combining thiol-modified concave-concave-concave-concave-concave-corrosion rock with nanozinc oxide, hydrothermal reaction is used to prepare nanotitanium dioxide to form a composite material with high specific surface area and wide bandgap, combining photocatalysis and adsorption. , realize effective degradation of methylene blue.

Benefits of technology

Under ultraviolet light irradiation, the composite material significantly improves the adsorption rate and degradation efficiency of methylene blue, avoids the loss of photocatalysts, expands the scope of use, and achieves efficient degradation of organic pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116943631B_ABST
    Figure CN116943631B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of photocatalysis, and discloses a nano titanium dioxide-zinc oxide composite material. In the process of preparing the nano titanium dioxide, mercapto-modified attapulgite and nano zinc oxide are added, and the nano titanium dioxide-zinc oxide composite material is prepared through a hydrothermal reaction. In the preparation process, amide groups and mercapto groups are introduced into the mercapto-modified attapulgite, which has a good adsorption effect on organic pollutants in wastewater. In the process of synthesizing the nano titanium dioxide, mercapto-modified attapulgite and nano zinc oxide are added, so that coupling and synergistic effects of two wide bandgap semiconductor materials, nano titanium dioxide and nano zinc oxide, are achieved, and the nano titanium dioxide and nano zinc oxide have a larger spectral absorption range, thereby improving the catalytic effect of the composite oxide of the nano titanium dioxide and the nano zinc oxide, and helping to improve the photodegradation activity of the composite material, thereby increasing the absorption rate of ultraviolet light and improving the efficiency of photocatalytic degradation of pollutants such as organic dyes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalysis, in particular to a nano titanium dioxide-zinc oxide composite material. Background Art

[0002] With the rapid development of industrialization in my country, more and more industrial wastewater is generated, which has attracted widespread attention and become an important issue that cannot be ignored. In the process of industrialization, the dye industry has developed rapidly, and various organic dyes have been put into the market one after another, generating a large amount of organic dye wastewater. As one of the most difficult to degrade industrial wastewaters, organic dye wastewater has the characteristics of deep chromaticity, high content of organic pollutants, high biological toxicity, complex composition and difficulty in degradation. Common organic pollutants include rhodamine B, methylene blue, methyl orange, etc., which are very harmful to human body and environment. How to treat organic dye wastewater in a green and efficient way has become a research hotspot.

[0003] Photocatalytic degradation technology has attracted wide attention as an ideal way to solve the problems of environmental pollution and energy shortage. Photocatalytic degradation uses radiation and highly active free radicals generated in the reaction system, and then degrades pollutants into corresponding inorganic substances through processes such as addition, substitution, and electron transfer between free radicals and organic pollutants. Chinese patent CN107486110B discloses a method for efficiently degrading methylene blue, preparing graphene / titanium dioxide hollow composite microspheres, and achieving the degradation of methylene blue under the action of ultraviolet light source high-pressure mercury lamp. It has efficient photocatalytic activity and lasting chemical stability, but the photocatalyst is not easy to recover and is prone to secondary environmental pollution. Chinese patent application CN103143324A discloses a guanidinobenzoate-modified attapulgite, which uses guanidinobenzoic acid hydrochloride to modify attapulgite to obtain guanidinobenzoic acid hydrochloride-modified attapulgite, with low production cost. The guanidinobenzoate-modified attapulgite is used to adsorb methylene blue in wastewater under mild adsorption conditions, without heating and in a short time, but its adsorption rate for methylene blue is low and cannot be degraded.

[0004] Therefore, it is urgent to develop a green and environmentally friendly composite material with high photocatalytic efficiency and adsorption effect. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a nano titanium dioxide-zinc oxide composite material, which is prepared by the following steps:

[0006] Anhydrous ethanol, titanium source, aqueous hydrogen peroxide solution, mercapto-modified attapulgite and nano zinc oxide are evenly mixed, acetic acid solution is added dropwise to adjust the pH to 4-5, and after stirring and mixing, a hydrothermal reaction is carried out in a polytetrafluoroethylene reactor. After the reaction is completed, centrifugal separation is carried out at a centrifugal rate of 8000r / min and a centrifugal time of 8min. The mixture is washed with deionized water and anhydrous ethanol, and vacuum dried at 60°C for 12h to obtain a nano titanium dioxide-zinc oxide composite material.

[0007] Preferably, the aqueous hydrogen peroxide solution is an aqueous hydrogen peroxide solution with a mass concentration of 10%.

[0008] Preferably, the temperature of the hydrothermal reaction is 125-135° C., and the time of the hydrothermal reaction is 12-15 h.

[0009] Preferably, the attapulgite is purchased from Xuyi Oubaite Clay Material Co., Ltd., and its main chemical composition is 63.2% SiO2, 12.5% ​​Al2O3, 8.9% MgO, 6.86% Fe2O3, 3.86% CaO, 1.9% K2O, and 0.15% Na2O.

[0010] Preferably, the titanium source includes any one of tetrabutyl titanate and ethyl titanate.

[0011] Preferably, the mass ratio of the anhydrous ethanol, the titanium source, the aqueous hydrogen peroxide solution, the mercapto-modified attapulgite and the nano zinc oxide is 1400-1600:305-340:520-580:100:90-105.

[0012] Preferably, the nano zinc oxide is prepared by the following steps:

[0013] Dissolve zinc acetate in deionized water, slowly add ammonia water, stir and mix, add sodium borohydride and polyvinyl pyrrolidone, mix well, and perform hydrothermal reaction in a polytetrafluoroethylene reactor. After the reaction is completed, cool, wash with anhydrous ethanol and deionized water, and vacuum dry at 60°C for 12 hours to obtain nano zinc oxide;

[0014] In the preparation process of the nano zinc oxide, the mass ratio of zinc acetate, deionized water, ammonia water, sodium borohydride and polyvinyl pyrrolidone is 100:4600:195:280:32;

[0015] The ammonia water is an aqueous solution of ammonia with a mass concentration of 10%;

[0016] During the preparation of the nano zinc oxide, the temperature of the hydrothermal reaction is 125° C. and the reaction time is 4 hours.

[0017] Preferably, the mercapto-modified attapulgite is prepared by the following steps:

[0018] Step 1, ultrasonically dispersing attapulgite (ATP) in toluene, after uniform dispersion, adding p-phenylene diisocyanate, stirring and mixing, reacting, centrifuging after the reaction, the centrifugal rate is 6000r / min, the centrifugal time is 8min, washing with ethyl acetate, drying in a vacuum drying oven at 60°C, the drying time is 12h, and obtaining isocyanate-modified attapulgite;

[0019] Step 2, ultrasonically dispersing the isocyanate-modified attapulgite in toluene, after uniform dispersion, adding 4-aminodiphenylethylene, stirring and mixing, heating, reacting, and centrifuging after the reaction is completed. The centrifugal rate is 6000r / min, and the centrifugal time is 8min. Washing with anhydrous ethanol, drying in a vacuum drying oven at 60°C, and the drying time is 12h, to obtain olefin-modified attapulgite;

[0020] Step three, ultrasonically disperse the olefin-modified attapulgite in anhydrous ethanol, and after uniform dispersion, add pentaerythritol tetrakis(thioglycolate) ester and an initiator, stir and mix, and react under ultraviolet light. After the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12 hours to obtain thiol-modified attapulgite.

[0021] Preferably, in the step 1, the mass ratio of attapulgite, toluene and p-phenylene diisocyanate is 100:3200-4000:65-90.

[0022] Preferably, the reaction temperature in step 1 is 25-35° C., and the reaction time is 12-15 h.

[0023] Preferably, in the step 2, the mass ratio of isocyanate-modified attapulgite, toluene and 4-aminostilbene is 100:2500-3000:130-180.

[0024] Preferably, the reaction temperature in step 2 is 85-98° C., and the reaction time is 8-10 h.

[0025] Preferably, in the step three, the mass ratio of olefin-modified attapulgite, anhydrous ethanol, pentaerythritol tetrakis(thioglycolate) ester and initiator is 100:1800-2400:105-135:0.2-0.5.

[0026] Preferably, the initiator in step three includes any one of 2-hydroxy-2-methylacetophenone and 2,2-dimethoxy-2-phenylacetophenone.

[0027] Preferably, the reaction temperature in step 3 is 20-30° C., and the reaction time is 2-3 h.

[0028] In the present invention, p-phenylene diisocyanate is first used to modify attapulgite, a hydroxyl group on the attapulgite reacts with an isocyanate on the p-phenylene diisocyanate to obtain isocyanate-modified attapulgite, an isocyanate group on the isocyanate-modified attapulgite reacts with an amino group on 4-aminostilbene to introduce a benzene ring and a carbon-carbon double bond to obtain olefin-modified attapulgite, and a click reaction occurs between the carbon-carbon double bond on the olefin-modified attapulgite and pentaerythritol tetrakis(thioglycolate) under the action of an initiator to obtain thiol-modified attapulgite.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The attapulgite in the present invention has a large specific surface area and a special physical and chemical structure and ionic state, and has excellent adsorption performance. Using attapulgite as a carrier of a photocatalyst avoids the problem of loss and difficulty in recovery of the photocatalyst during use, thereby expanding the scope of use. The attapulgite is modified to introduce more active sites, thereby better adsorbing organic pollutants in wastewater. A large number of amide groups and sulfhydryl groups are introduced during the reaction process, which have a good adsorption effect on organic pollutants in wastewater. Among them, when a large number of sulfhydryl groups are introduced, the sulfhydryl groups lose proton hydrogen during the adsorption process to form sulfhydryl anions, and methylene blue is a cationic dye, which generates electrostatic attraction with sulfur anions, thereby achieving a good electrostatic adsorption effect on methylene blue. The introduced amide groups can form hydrogen bonds and coupling effects with dye molecules, providing more active adsorption sites.

[0031] (2) In the present invention, mercapto-modified attapulgite and nano zinc oxide are added during the synthesis of nano titanium dioxide, and nano titanium dioxide can be uniformly grown on the attapulgite carrier. Both nano titanium dioxide and zinc oxide have large specific surface areas. There is a certain band gap between the conduction band and the valence band of nano zinc oxide. When exposed to light, when the light energy is greater than the band gap, the electrons in the valence band are excited and thus jump to the conduction band, leaving holes in the valence band. The electron-hole pairs further combine with the groups in water to form ·O 2- When nano-titanium dioxide is irradiated by ultraviolet light, the electrons in the valence band are excited and jump to the conduction band to form photogenerated electrons. The photogenerated electrons and holes migrate to the surface of titanium dioxide, showing excellent photocatalytic activity, so that methylene blue is oxidized into small molecules, effectively degrading methylene blue in water.

[0032] (3) In the present invention, mercapto-modified attapulgite and nano-zinc oxide are added during the synthesis of nano-titanium dioxide. Nano-titanium dioxide can grow evenly on the attapulgite carrier. The attapulgite quickly adsorbs organic pollutants, accelerates the photodegradation rate of the photocatalyst, and simultaneously realizes the coupling and synergistic effect of two wide-bandgap semiconductor materials, nano-titanium dioxide and nano-zinc oxide, with a larger spectral absorption range, thereby improving the catalytic effect of the composite oxide of nano-titanium dioxide and nano-zinc oxide, and helping to improve the photodegradation activity of the composite material, thereby increasing the absorption rate of ultraviolet light and improving the efficiency of photocatalytic degradation of pollutants such as organic dyes. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the reaction of isocyanate-modified attapulgite in the present invention;

[0034] Figure 2 Schematic diagram of the reaction of olefin-modified attapulgite in the present invention;

[0035] Figure 3 It is a schematic diagram of the reaction of mercapto-modified attapulgite modification in the present invention. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] A nano titanium dioxide-zinc oxide composite material is prepared by the following steps:

[0039] Anhydrous ethanol, tetrabutyl titanate, aqueous hydrogen peroxide solution, mercapto-modified attapulgite and nano zinc oxide in a mass ratio of 1400:305:520:100:90 were evenly mixed, acetic acid solution was added dropwise to adjust the pH to 4, and after stirring and mixing, a hydrothermal reaction was carried out at 125°C in a polytetrafluoroethylene reactor for 12 hours. After the reaction was completed, centrifugal separation was carried out at a rate of 8000 r / min for 8 minutes. The mixture was washed with deionized water and anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain a nano titanium dioxide-zinc oxide composite material.

[0040] The mercapto-modified attapulgite is prepared by the following steps:

[0041] Step 1, ultrasonically disperse the attapulgite in toluene, and after uniform dispersion, add p-phenylene diisocyanate, wherein the mass ratio of attapulgite, toluene and p-phenylene diisocyanate is 100:3200:65, stir and mix, react at 25°C, and the reaction time is 12h. After the reaction is completed, centrifuge at a rate of 6000r / min and a centrifugation time of 8min, wash with ethyl acetate, and dry in a vacuum drying oven at 60°C for 12h to obtain isocyanate-modified attapulgite;

[0042] Step 2, ultrasonically dispersing the isocyanate-modified attapulgite in toluene, and after uniform dispersion, adding 4-aminostilbene, wherein the mass ratio of isocyanate-modified attapulgite, toluene, and 4-aminostilbene is 100:2500:130, stirring and mixing, heating, reacting at 85°C for 8 hours, and after the reaction is completed, centrifuging at a rate of 6000r / min for 8 minutes, washing with anhydrous ethanol, and drying in a vacuum drying oven at 60°C for 12 hours to obtain olefin-modified attapulgite;

[0043] Step three, ultrasonically disperse the olefin-modified attapulgite in anhydrous ethanol, and after uniform dispersion, add pentaerythritol tetrakis(thioglycolic acid) ester and initiator 2-hydroxy-2-methylpropiophenone, wherein the mass ratio of olefin-modified attapulgite, anhydrous ethanol, pentaerythritol tetrakis(thioglycolic acid) ester and initiator 2-hydroxy-2-methylpropiophenone is 100:1800:105:0.2, stir and mix, react at 20°C under ultraviolet light, and the reaction time is 2h. After the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain thiol-modified attapulgite.

[0044] Example 2

[0045] A nano titanium dioxide-zinc oxide composite material is prepared by the following steps:

[0046] Anhydrous ethanol, tetrabutyl titanate, aqueous hydrogen peroxide solution, mercapto-modified attapulgite and nano zinc oxide in a mass ratio of 1480:320:540:100:95 were evenly mixed, acetic acid solution was added dropwise to adjust the pH to 4.5, and after stirring and mixing, a hydrothermal reaction was carried out in a polytetrafluoroethylene reactor at 130°C for 14 hours. After the reaction was completed, centrifugal separation was carried out at a centrifugal speed of 8000 r / min for 8 minutes. The nano titanium dioxide-zinc oxide composite material was washed with deionized water and anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain.

[0047] The mercapto-modified attapulgite is prepared by the following steps:

[0048] Step 1, ultrasonically disperse the attapulgite in toluene, and after uniform dispersion, add p-phenylene diisocyanate, wherein the mass ratio of attapulgite, toluene and p-phenylene diisocyanate is 100:3800:80, stir and mix, react at 30°C, and the reaction time is 14h. After the reaction is completed, centrifuge at a rate of 6000r / min and a centrifugation time of 8min, wash with ethyl acetate, and dry in a vacuum drying oven at 60°C for 12h to obtain isocyanate-modified attapulgite;

[0049] Step 2, ultrasonically dispersing the isocyanate-modified attapulgite in toluene, and after uniform dispersion, adding 4-aminostilbene, wherein the mass ratio of isocyanate-modified attapulgite, toluene, and 4-aminostilbene is 100:2800:160, stirring and mixing, heating, reacting at 95°C for 9 hours, and centrifuging after the reaction, at a centrifugal rate of 6000r / min, for 8 minutes, washing with anhydrous ethanol, and drying in a vacuum drying oven at 60°C for 12 hours to obtain olefin-modified attapulgite;

[0050] Step three, ultrasonically disperse the olefin-modified attapulgite in anhydrous ethanol, and after uniform dispersion, add pentaerythritol tetrakis(thioglycolate) ester and initiator 2-hydroxy-2-methylpropiophenone, wherein the mass ratio of olefin-modified attapulgite, anhydrous ethanol, pentaerythritol tetrakis(thioglycolate) ester and initiator 2-hydroxy-2-methylpropiophenone is 100:2200:120:0.4, stir and mix, react at 25°C under ultraviolet light, and the reaction time is 2.5h. After the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain thiol-modified attapulgite.

[0051] Example 3

[0052] A nano titanium dioxide-zinc oxide composite material is prepared by the following steps:

[0053] Anhydrous ethanol, tetrabutyl titanate, aqueous hydrogen peroxide solution, mercapto-modified attapulgite and nano zinc oxide in a mass ratio of 1550:330:560:100:100 were evenly mixed, acetic acid solution was added dropwise to adjust the pH to 4.5, and after stirring and mixing, a hydrothermal reaction was carried out in a polytetrafluoroethylene reactor at 130°C for 14 hours. After the reaction was completed, centrifugal separation was carried out at a rate of 8000 r / min for 8 minutes, and the mixture was washed with deionized water and anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain a nano titanium dioxide-zinc oxide composite material.

[0054] The preparation method of the mercapto-modified attapulgite is the same as the preparation method of the mercapto-modified attapulgite in Example 2.

[0055] Example 4

[0056] A nano titanium dioxide-zinc oxide composite material is prepared by the following steps:

[0057] Anhydrous ethanol, tetrabutyl titanate, aqueous hydrogen peroxide solution, mercapto-modified attapulgite and nano zinc oxide in a mass ratio of 1600:340:580:100:105 were evenly mixed, acetic acid solution was added dropwise to adjust the pH to 5, and after stirring and mixing, a hydrothermal reaction was carried out at 135°C in a polytetrafluoroethylene reactor for 15 hours. After the reaction was completed, centrifugal separation was carried out at a centrifugal speed of 8000 r / min for 8 minutes. The mixture was washed with deionized water and anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain a nano titanium dioxide-zinc oxide composite material.

[0058] The mercapto-modified attapulgite is prepared by the following steps:

[0059] Step 1, ultrasonically disperse the attapulgite in toluene, and after uniform dispersion, add p-phenylene diisocyanate, wherein the mass ratio of attapulgite, toluene and p-phenylene diisocyanate is 100:4000:90, stir and mix, react at 35°C for 15 hours, and after the reaction is completed, centrifuge at a rate of 6000r / min for 8 minutes, wash with ethyl acetate, and dry in a vacuum drying oven at 60°C for 12 hours to obtain isocyanate-modified attapulgite;

[0060] Step 2, ultrasonically dispersing the isocyanate-modified attapulgite in toluene, and after uniform dispersion, adding 4-aminostilbene, wherein the mass ratio of isocyanate-modified attapulgite, toluene, and 4-aminostilbene is 100:3000:180, stirring and mixing, heating, reacting at 98°C for 10 hours, and centrifuging after the reaction, at a rate of 6000r / min, for 8 minutes, washing with anhydrous ethanol, and drying in a vacuum drying oven at 60°C for 12 hours to obtain olefin-modified attapulgite;

[0061] Step three, ultrasonically disperse the olefin-modified attapulgite in anhydrous ethanol, and after uniform dispersion, add pentaerythritol tetrakis(thioglycolic acid) ester and initiator 2-hydroxy-2-methylpropiophenone, wherein the mass ratio of olefin-modified attapulgite, anhydrous ethanol, pentaerythritol tetrakis(thioglycolic acid) ester and initiator 2-hydroxy-2-methylpropiophenone is 100:2400:135:0.5, stir and mix, react at 30°C under ultraviolet light, and the reaction time is 3h. After the reaction is completed, filter, wash with anhydrous ethanol, and dry in a drying oven at 80°C for 12h to obtain thiol-modified attapulgite.

[0062] Comparative Example 1

[0063] A nano titanium dioxide-zinc oxide composite material is prepared by the following steps:

[0064] Anhydrous ethanol, tetrabutyl titanate, aqueous hydrogen peroxide solution, attapulgite and nano zinc oxide in a mass ratio of 1550:330:560:100:100 were evenly mixed, acetic acid solution was added dropwise to adjust the pH to 4.5, and after stirring and mixing, a hydrothermal reaction was carried out at 130°C in a polytetrafluoroethylene reactor for 14 hours. After the reaction was completed, centrifugal separation was carried out at a rate of 8000 r / min for 8 minutes. The mixture was washed with deionized water and anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain a nano titanium dioxide-zinc oxide composite material.

[0065] Comparative Example 2

[0066] A nano titanium dioxide composite material is prepared by the following steps:

[0067] Anhydrous ethanol, tetrabutyl titanate, aqueous hydrogen peroxide solution and mercapto-modified attapulgite in a mass ratio of 1550:330:560:100 were uniformly mixed, acetic acid solution was added dropwise to adjust the pH to 4.5, and after stirring and mixing, a hydrothermal reaction was carried out in a polytetrafluoroethylene reactor at 130° C. The hydrothermal reaction time was 14 hours. After the reaction was completed, centrifugal separation was performed at a centrifugal speed of 8000 r / min and a centrifugal time of 8 minutes. Deionized water and anhydrous ethanol were used for washing, and vacuum drying was performed at 60° C. for 12 hours to obtain a nano-titanium dioxide composite material;

[0068] The preparation method of the mercapto-modified attapulgite is the same as the preparation method of the mercapto-modified attapulgite in Example 2.

[0069] Comparative Example 3

[0070] A nano titanium dioxide-zinc oxide composite material is prepared by the following steps:

[0071] Anhydrous ethanol, nano-titanium dioxide, aqueous hydrogen peroxide solution, mercapto-modified attapulgite and nano-zinc oxide in a mass ratio of 1550:78:560:100:100 were uniformly mixed, acetic acid solution was added dropwise to adjust the pH to 4.5, and after stirring and mixing, a hydrothermal reaction was carried out in a polytetrafluoroethylene reactor at 130° C. The hydrothermal reaction time was 14 h. After the reaction was completed, centrifugation was performed at a rate of 8000 r / min for 8 min, and the mixture was washed with deionized water and anhydrous ethanol, and vacuum dried at 60° C. for 12 h to obtain a nano-titanium dioxide-zinc oxide composite material;

[0072] The nano titanium dioxide was purchased from Nanjing Baoket New Materials Co., Ltd., model PTT-GA10, with an average particle size of 10 nm.

[0073] The preparation method of the mercapto-modified attapulgite is the same as the preparation method of the mercapto-modified attapulgite in Example 2.

[0074] The composite materials prepared in Examples 1-4 and Comparative Examples 1-3 were selected as samples and performance tests were performed as follows:

[0075] 200 mL of a 50 mg / L methylene blue solution was added to the reaction tube, and 0.5 g of the samples prepared in Examples 1-4 and Comparative Examples 1-3 were added as catalysts, respectively, and stirred in a dark place for 0.5 h. The concentration of the reaction solution was tested, and the adsorption rate was calculated. The reaction was then placed in a photocatalytic reactor, and a constant flow of air was introduced. A 300 W high-pressure mercury lamp was used as an ultraviolet light source, and the wavelength of the light was 365 nm. The vertical distance between the light source and the solution was 10 cm. After the photoreaction, 5 mL of the dispersion was removed from the reaction system every 30 min and placed in a centrifuge tube. The supernatant was taken, and the absorbance and concentration of methylene blue in the solution were tested using a U3900 UV-visible spectrophotometer. The degradation rate after treatment was calculated, wherein D = (C0-C) / C0 = (A0-A) / A0 × 100%, wherein D is the degradation rate, C0, C, A0, and A represent the initial concentration of the solution and the concentration after treatment, the initial absorbance, and the absorbance after treatment, respectively. The test results are shown in Table 1:

[0076] Table 1

[0077]

[0078]

[0079] According to the test results in Table 1, it can be seen that Examples 1-4 have excellent adsorption and photocatalytic properties for methylene blue. After 0.5 h of adsorption, the composite material corresponding to Example 4 has an adsorption rate of 73.5%, a degradation rate of 94.5% after 1 h of photodegradation, and a degradation rate of 99.6% after 3 h of photodegradation, and has a strong methylene blue removal ability. The attapulgite in comparative example 1 has not been modified by thiol group, and its adsorption performance is greatly reduced. After the corresponding composite material is adsorbed for 0.5h, the adsorption rate is 42.7%, the degradation rate is 75.4% after 1h of photodegradation, and the degradation rate can reach 91.7% after 3h of photodegradation; in comparative example 2, no nano zinc oxide is added, which has little effect on the adsorption rate of light-avoiding adsorption. After the corresponding composite material is adsorbed for 0.5h, the adsorption rate can reach 71.3%, which has a great effect on the light degradation rate, the degradation rate can reach 78.7% after 1h of photodegradation, and the degradation rate can reach 85.4% after 3h of photodegradation; in comparative example 3, nano titanium dioxide is commercially available, which has little effect on the adsorption rate of light-avoiding adsorption. After the corresponding composite material is adsorbed for 0.5h, the adsorption rate can reach 71.9%, and the effect on the light degradation rate is also small, the degradation rate can reach 87.8% after 1h of photodegradation, and the degradation rate can reach 94.3% after 3h of photodegradation.

[0080] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A nano titanium dioxide-zinc oxide composite material, characterized in that: The nano titanium dioxide-zinc oxide composite material is prepared by the following steps: The anhydrous ethanol, titanium source, hydrogen peroxide aqueous solution, mercapto-modified attapulgite and nano zinc oxide were uniformly mixed, acetic acid solution was added dropwise to adjust the pH to 4-5, the mixture was stirred and mixed, and a hydrothermal reaction was performed. After the reaction was completed, the mixture was centrifuged at a rate of 8000 r / min for 8 min, and the mixture was washed with deionized water and anhydrous ethanol, and vacuum dried at 60° C. for 12 h to obtain a nano titanium dioxide-zinc oxide composite material. The aqueous hydrogen peroxide solution is an aqueous hydrogen peroxide solution with a mass concentration of 10%; The temperature of the hydrothermal reaction is 125-135°C, and the time of the hydrothermal reaction is 12-15h; The preparation method of the mercapto-modified attapulgite comprises the following steps: Step 1, ultrasonically dispersing the attapulgite in toluene, after uniform dispersion, adding p-phenylene diisocyanate, stirring and mixing, reacting, and after the reaction is completed, centrifuging at a rate of 6000 r / min for 8 min, washing with ethyl acetate, and drying in a vacuum drying oven at 60° C. for 12 h to obtain isocyanate-modified attapulgite; Step 2, ultrasonically dispersing the isocyanate-modified attapulgite in toluene, after uniform dispersion, adding 4-aminodiphenylethylene, stirring and mixing, heating, reacting, and centrifuging after the reaction is completed. The centrifugal rate is 6000r / min, and the centrifugal time is 8min. Washing with anhydrous ethanol, drying in a vacuum drying oven at 60°C, and the drying time is 12h, to obtain olefin-modified attapulgite; Step 3, ultrasonically dispersing the olefin-modified attapulgite in anhydrous ethanol, adding pentaerythritol tetrakis(thioglycolate) ester and an initiator after uniform dispersion, stirring and mixing, reacting under ultraviolet light, filtering after the reaction, washing with anhydrous ethanol, and drying in a drying oven at 80° C. for 12 h to obtain thiol-modified attapulgite; In the step 2, the mass ratio of isocyanate-modified attapulgite, toluene and 4-aminostilbene is 100:2500-3000:130-180; In the step three, the mass ratio of olefin-modified attapulgite, anhydrous ethanol, pentaerythritol tetrakis(thioglycolate) ester and initiator is 100:1800-2400:105-135:0.2-0.

5.

2. A nano titanium dioxide-zinc oxide composite material according to claim 1, characterized in that: The titanium source is selected from any one of tetrabutyl titanate and ethyl titanate.

3. A nano titanium dioxide-zinc oxide composite material according to claim 1, characterized in that: The mass ratio of the anhydrous ethanol, the titanium source, the hydrogen peroxide aqueous solution, the mercapto-modified attapulgite and the nano zinc oxide is 1400-1600:305-340:520-580:100:90-105.

4. The nano titanium dioxide-zinc oxide composite material according to claim 1, characterized in that: The reaction temperature in step 2 is 85-98° C., and the reaction time is 8-10 h.

5. The nano titanium dioxide-zinc oxide composite material according to claim 1, characterized in that: In the step three, the initiator is selected from any one of 2-hydroxy-2-methylacetophenone and 2,2-dimethoxy-2-phenylacetophenone.

6. The nano titanium dioxide-zinc oxide composite material according to claim 1, characterized in that: The reaction temperature in step 3 is 20-30° C., and the reaction time is 2-3 h.