A beryllium ultra-stable mineralization reagent and a method for ultra-stable mineralization of dangerous beryllium elements in lithium slag
By using beryllium super-stable mineralization reagent combined with phosphate and calcium compounds and fluoride during lithium smelting, the dangerous beryllium elements in the lithium slag are converted into stable minerals, and the problem of beryllium pollution during lithium smelting is solved and the problem of beryllium pollution during lithium smelting is achieved. Low toxicity treatment and resource utilization of beryllium in lithium slag.
Patent Information
- Application Number
- CN202310894894.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-07-20
AI Technical Summary
The toxicity of dangerous beryllium element leaching in lithium slag produced during lithium smelting exceeds the standard, and the existing technology lacks effective stabilization methods, resulting in limited environmental pollution and resource utilization.
Using beryllium super-stable mineralization reagents combined with phosphate and/or calcium compounds and fluorides, the free beryllium is converted into stable minerals such as beryllium hydroxy phosphate, beryllium fluorine phosphate and calcium fluorine leachate, and the leaching of beryllium is reduced through mineralization reaction. toxicity.
The long-term ultra-stable mineralization of beryllium in lithium slag is achieved, which reduces the beryllium leaching toxicity of the lithium slag after treatment, meets the national hazardous waste leaching standards, and is simple, economical and efficient in the process, avoiding secondary pollution.
Smart Images

Figure BDA0004349415790000051 
Figure BDA0004349415790000062 
Figure BDA0004349415790000071
Abstract
Description
Technical Field
[0001] The invention relates to a beryllium ultra-stable mineralization reagent and also relates to a method for ultra-stable mineralization of dangerous beryllium elements in lithium slag, in particular to a method for long-term stabilization of beryllium elements in leached slag during the smelting process of lepidolite and spodumene, belonging to the technical field of beryllium pollution prevention and control. Background Art
[0002] In recent years, with the continuous growth of lithium demand, lithium-rich minerals such as lepidolite and spodumene have become industrial raw materials for lithium extraction. The enrichment of lepidolite or spodumene from low-grade lithium ore to produce lithium concentrate will produce a large amount of tailings slag. With the rapid development of my country's lithium industry, my country produced 240,000 tons of lithium carbonate and 175,000 tons of lithium hydroxide in 2021. It is estimated that 10 to 20 tons of lithium smelting slag will be produced for every ton of lithium carbonate or lithium hydroxide produced. The total amount of lithium smelting slag for the whole year is as high as 6 million tons. Against the background of the booming lithium industry, how to deal with lithium smelting slag has become an important constraint on the healthy development of the lithium industry.
[0003] Due to the affinity principle of earth elements, basically all lithium ores contain a certain amount of beryllium-containing minerals. In the smelting process of lithium ore, such as sodium chloride pressure cooking process, roasting water leaching process, high acid leaching process, etc., the lattice structure of beryllium-containing minerals is destroyed at the same time, which significantly increases the activity of beryllium in lithium slag. In the solid waste leaching toxicity test of lithium slag, the concentration of beryllium in the leachate can be as high as 10mg / L, far exceeding the national standard of 0.02mg / L. Beryllium and its compounds are highly toxic, soluble beryllium is highly toxic, and insoluble beryllium is less toxic. Therefore, lithium slag must be treated to reduce the leaching toxicity of beryllium before it can be disposed of or recycled. However, at present, there is almost no stabilization technology for dangerous beryllium elements in lithium slag. Summary of the invention
[0004] In view of the problem of excessive toxicity of dangerous beryllium elements leached out of lithium slag produced in the lithium ore smelting process in the prior art, the first purpose of the present invention is to provide a beryllium ultra-stable mineralization reagent, which can mineralize free beryllium into stable minerals such as hydroxyberyllium phosphate, beryllium fluorophosphate and calcium fluoroberyllate, thereby achieving long-term ultra-stable mineralization of free beryllium and reducing beryllium pollution in the environment.
[0005] The second object of the present invention is to provide a method for ultra-stable mineralization of hazardous beryllium elements in lithium slag. The method utilizes a beryllium ultra-stable mineralization reagent to achieve ultra-stabilization of free beryllium (mainly non-stable beryllium, including beryllium cations and beryllium-containing anions) in lithium slag, so that the leaching toxicity of beryllium in the treated lithium slag under natural storage conditions is lower than the national standard for toxic leaching of hazardous waste.
[0006] In order to achieve the above technical objectives, the present invention provides a beryllium ultra-stable mineralization reagent, which includes phosphate and / or calcium compound and fluoride.
[0007] The beryllium ultra-stable mineralization reagent provided by the technical solution of the present invention includes phosphate and / or calcium compound and fluoride, fluoride provides fluoride ion, which is a necessary component of the beryllium ultra-stable mineralization reagent, while phosphate and calcium compound provide phosphate and calcium ion respectively, which are optional components, mainly based on the significant amphoteric properties of beryllium element, and the mineralization principle is completely different for beryllium in different states of existence. The technical solution of the present invention is based on the principle that the properties of beryllium cations are similar to calcium ions and magnesium ions, and the properties of beryllium-containing anions are similar to silicate and phosphate, and beryllium cations are used to convert into hydroxy beryllium phosphate and beryllium fluorophosphate with a stable apatite configuration, and beryllium-containing anions are used to convert into calcium fluoroberylate with a stable calcium fluorosilicate configuration. Therefore, by selecting phosphate and / or calcium compounds and fluoride for use in combination, beryllium in different states of existence can be effectively ultra-stabilized.
[0008] As a preferred solution, the phosphate mainly provides phosphate radicals, and general soluble phosphates meet the application requirements. Common phosphates include at least one of sodium phosphate and potassium phosphate.
[0009] As a preferred solution, the calcium compound mainly provides calcium ions, and general soluble calcium compounds meet the application requirements. The calcium compound includes at least one of calcium carbonate, calcium hydroxide, and calcium oxide.
[0010] As a preferred solution, the fluoride mainly provides fluoride ions, and general soluble fluorides meet the application requirements. The fluoride includes at least one of calcium fluoride, sodium fluoride, potassium fluoride, and hydrofluoric acid.
[0011] As a preferred solution, the beryllium ultra-stable mineralization reagent contains the following components by mass: 1 to 5 parts of phosphate; 1 to 2 parts of calcium compound; 1 to 2 parts of fluoride. The preferred beryllium ultra-stable mineralization reagent can simultaneously mineralize amphoteric beryllium ions, and beryllium cations are mainly converted into stable hydroxy beryllium phosphate and beryllium fluorophosphate with phosphate ions and fluoride ions, while beryllium anions are mainly converted into stable calcium fluoroberyllate with calcium ions and fluoride ions. The ratio of phosphate, calcium compound and fluoride in the beryllium ultra-stable mineralization reagent is mainly determined based on the ratio of anion and cation forms of free beryllium in lithium slag. For example, when there are more beryllium cations, phosphate and fluoride are mainly added; if there are more beryllium anions, fluoride and calcium compound are mainly added. It is best to use the three agents of phosphate, calcium compound and fluoride in coordination to ensure the long-term stabilization of free beryllium. The mass ratio of the phosphate, the calcium compound and the fluoride is more preferably (2 to 4):(1 to 2):(1 to 2).
[0012] As a preferred solution, the beryllium ultra-stable mineralization reagent comprises the following components by weight: 1 to 5 parts of phosphate; 1 part of fluoride. The preferred beryllium ultra-stable mineralization reagent can mineralize beryllium cations, and beryllium cations are mainly converted into stable hydroxy beryllium phosphate and fluoro beryllium phosphate with phosphate ions and fluoride ions. The stability of fluoro beryllium phosphate is higher than that of hydroxy beryllium phosphate, so the ratio of phosphate to fluoride is controlled within an appropriate range, so that the mineralization product mainly exists in the form of fluoro beryllium phosphate. If the phosphate is greatly excessive, the proportion of hydroxy beryllium phosphate in the mineralization product is too high, and when the proportion of fluoride is too high, beryllium fluoride with poor stability will be formed. Therefore, the ratio of phosphate to fluoride is preferably controlled at (1 to 3): 1.
[0013] As a preferred solution, the beryllium ultra-stable mineralization reagent comprises the following components by mass: 1 to 2 parts of calcium compound; 1 part of fluoride. The preferred beryllium ultra-stable mineralization reagent can mineralize beryllium-containing anions, and the beryllium-containing anions are mainly converted into stable calcium fluoroberyllate with calcium ions and fluoride ions. If free beryllium exists in the form of beryllium-containing anions, it is necessary to first add fluoride to convert the beryllium-containing anions into fluoroberyllate, and then add calcium compounds to form calcium fluoroberyllate precipitation using calcium ions and fluoroberyllate. If the ratio of calcium compounds is too low, the fluoroberyllate cannot be completely converted, and if the ratio of fluorides is too low, the beryllium-containing anions cannot be completely converted into calcium fluoroberyllate. Excessive calcium compounds and fluorides do not contribute to the fixation of beryllium-containing anions, so it is further preferred that the ratio of calcium compounds to fluorides is controlled at (1.5 to 2): 1.
[0014] The present invention also provides a method for ultra-stable mineralization of dangerous beryllium elements in lithium slag. The method comprises slurrying the ultra-stable beryllium mineralization reagent, adding the slurried lithium slag or lithium mineral leaching slurry to carry out a mineralization reaction, and after the mineralization reaction is completed, filtering and separating to obtain ultra-stable mineralized lithium slag.
[0015] As a preferred solution, phosphate and fluoride are mixed and slurried, and then added to slurried lithium slag or lithium mineral leaching slurry, and stirred for mineralization reaction; wherein the mass ratio of phosphate to fluoride is (1-5):1, the total mass of phosphate and fluoride is 2.0%-7.0% of the mass of lithium slag in slurried lithium slag or lithium mineral leaching slurry, and the mass of water in slurried lithium slag accounts for 40%-200% of the mass of lithium slag. Stirring can strengthen the full contact reaction between lithium slag and reagent.
[0016] As a preferred solution, after fluoride is slurried, it is added to the slurried lithium slag or lithium mineral leaching slurry and stirred for mineralization reaction, and then the calcium compound is slurried and added to the slurried lithium slag or lithium mineral leaching slurry to continue the mineralization reaction; wherein, the mass ratio of fluoride to calcium compound is 1:(1-2), and the total mass of fluoride and calcium compound is 3.0%-10.0% of the mass of lithium slag in the slurried lithium slag or lithium mineral leaching slurry; the mass of water in the slurried lithium slag accounts for 40%-200% of the mass of lithium slag. Fluoride is added first, and calcium compound is added later, mainly because there is competition between calcium ions and beryllium cations, and calcium ions will be converted into calcium fluoride precipitation with fluoride ions, consuming the added fluoride ions, therefore, the subsequent addition of calcium compound is conducive to the formation of very stable calcium fluoroberyllate, and keeps the lithium slag neutral or weakly alkaline to prevent beryllium leaching.
[0017] As a preferred solution, phosphate and fluoride are mixed and slurried, and then added to the slurried lithium slag or lithium mineral leaching slurry, stirred for mineralization reaction, and then the calcium compound is slurried and applied to the slurried lithium slag or lithium mineral leaching slurry to continue the mineralization reaction, the mass ratio of phosphate, fluoride and calcium compound is (1-5): (1-2): (1-2), the total mass of phosphate, fluoride and calcium compound is 1%-8% of the mass of lithium slag in the slurried lithium slag or lithium mineral leaching slurry, and the mass of water in the slurried lithium slag accounts for 40%-200% of the mass of lithium slag. Phosphate and fluoride are added first, and calcium compound is added later, mainly because there is competition between calcium ions and beryllium cations, calcium ions preferentially react with fluoride ions and phosphate ions to form calcium phosphate and calcium fluoride precipitation, consuming the added phosphate and fluoride ions, and the subsequent addition of calcium compound is conducive to the formation of very stable calcium fluoroberyllate, and keeps the lithium slag neutral or weakly alkaline to prevent beryllium leaching.
[0018] As a preferred solution, the temperature of the mineralization reaction is room temperature, and the total time is 20 to 60 minutes.
[0019] As a preferred solution, the filtrate obtained by filtration separation is recycled, the filter residue obtained by filtration separation is washed with water, and the washing liquid is recycled. When the salt content in the filtrate and the washing liquid is too high, a partial volume of solution needs to be opened for purification and discharge.
[0020] The lithium slag of the present invention is solid waste generated during the smelting process of lepidolite and spodumene, mainly including leached slag of roasted materials, etc. Since lepidolite, spodumene and other lithium ores are often associated with beryllium-containing minerals such as beryl and chrysoberyl, the leaching toxicity of beryllium element (a type of pollutant) in the lithium slag exceeds the national standard, resulting in serious restrictions on the storage and disposal of lithium slag.
[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0022] 1) The stabilization technology of hazardous beryllium elements in lithium slag in the prior art has not been developed, and there is a technical gap. The technical solution of the present invention proposes for the first time a method for ultra-stable mineralization of beryllium in lithium slag. By utilizing the combination of common phosphates, calcium compounds and fluorides in the prior art, free beryllium, especially free beryllium cations and beryllium anions, can be mineralized into stable minerals such as hydroxyberyllium phosphate, beryllium fluorophosphate and calcium fluoroberyllate, thereby realizing long-term ultra-stable mineralization of free beryllium, which can effectively solve the practical problem of beryllium pollution in the lithium smelting process.
[0023] 2) The beryllium ultra-stable mineralizing agent proposed in the technical solution of the present invention is a conventional chemical product, which has the advantages of being cheap, easy to obtain, easy to store and use, and having no secondary pollution.
[0024] 3) The beryllium ultra-stable mineralization construction process proposed in the technical solution of the present invention is simple and efficient, does not require complex and expensive equipment and instruments, and the overall operation process has the advantages of being economical, efficient, and easy to implement. DETAILED DESCRIPTION
[0025] The following examples are provided to further illustrate the present invention, but are not intended to limit the scope of protection of the claims of the present invention.
[0026] Example 1
[0027] The method of the present invention is used to treat lithium slag produced by a lithium smelting enterprise in Hunan, wherein the beryllium content in the lithium slag is 0.051% (through chemical titration analysis, the beryllium cation accounts for 98.75% and the beryllium anion accounts for 1.25%), and the water content is 16.44%. The slag is subjected to leaching toxicity test according to the standards of "Identification Standard for Hazardous Waste Leaching Toxicity Identification (GB 5085.3-2007)" and "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method (HJ / T 299-2007)", and the results show that the beryllium content in the leachate is 5.22 mg / L, which exceeds the national standard of 0.02 mg / L. The treatment process of ultra-stable mineralization of beryllium in lithium slag is briefly described as follows: prepare 10% sodium phosphate, sodium fluoride, and calcium hydroxide solution or suspension respectively, add 50% water by mass to the lithium slag for slurrying, and then add 2% sodium phosphate (the percentage of sodium phosphate relative to the dry weight of lithium slag) and 1% sodium fluoride (the percentage of sodium fluoride relative to the dry weight of lithium slag) by mass to the slurry lithium slag, mechanically stir for 30 minutes, and then add 2% calcium hydroxide by mass, and then mechanically stir for 30 minutes to end the stabilization reaction. After filtering and washing the stabilized lithium slag, the leaching toxicity of the treated lithium slag is tested, and the beryllium content in multiple batches of leachate is 0.003-0.005 mg / L, which is lower than the national standard.
[0028] The following table shows the treatment effect of beryllium ultra-stable mineralizing reagent composed of different amounts of sodium phosphate, sodium fluoride and calcium hydroxide on lithium slag (refer to Example 1 for specific operation):
[0029]
[0030]
[0031] Example 2
[0032] The method of the present invention is applied to treat lithium slag produced by a lithium smelting enterprise in Jiangxi Province, wherein the beryllium content in the lithium slag is 0.02% (through chemical titration analysis, the proportion of beryllium cations is 99.63%, and the proportion of beryllium anions is 0.37%), and the water content is 12.31%. The slag is subjected to leaching toxicity test according to the standards of "Identification Standard for Hazardous Waste Leaching Toxicity Identification (GB 5085.3-2007)" and "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method (HJ / T 299-2007)", and the results show that the beryllium content in the leachate is 2.14 mg / L, which exceeds the national standard of 0.02 mg / L. The treatment process of ultra-stable mineralization of beryllium in lithium slag is briefly described as follows: prepare 10% sodium phosphate solution, sodium fluoride solution, and calcium carbonate suspension respectively, add 50% water by mass to the lithium slag for slurrying, and then add 2% sodium phosphate (the percentage of sodium phosphate relative to the dry weight of lithium slag) and 0.5% sodium fluoride (the percentage of sodium fluoride relative to the dry weight of lithium slag) by mass to the slurry lithium slag, mechanically stir for 30 minutes, and then add 0.5% calcium carbonate (the percentage of calcium carbonate relative to the dry weight of lithium slag) by mass to the slurry lithium slag, and then mechanically stir for 30 minutes before the stabilization reaction ends. After filtering and washing the stabilized lithium slag, the leaching toxicity of the treated lithium slag is tested, and the beryllium content in multiple batches of leachate is 0.01-0.02 mg / L, which is lower than the national standard.
[0033] The following table shows the treatment effect of beryllium ultra-stable mineralizing reagent composed of different amounts of sodium phosphate, sodium fluoride and calcium carbonate on lithium slag (refer to Example 2 for specific operation):
[0034]
[0035] Example 3
[0036] The method of the present invention is applied to treat lithium slag produced by a lithium smelting enterprise in Sichuan, wherein the beryllium content in the lithium slag is 0.07% (through chemical titration analysis, the beryllium cation accounts for 81.28%, and the beryllium anion accounts for 18.72%), and the water content is 19.74%. The slag is subjected to leaching toxicity test according to the standards of "Identification Standard for Hazardous Waste Leaching Toxicity Identification (GB 5085.3-2007)" and "Solid Waste Leaching Toxicity Leaching Method Sulfuric Acid and Nitric Acid Method (HJ / T 299-2007)", and the results show that the beryllium content in the leachate is 4.28 mg / L, which exceeds the national standard of 0.02 mg / L. The treatment process of ultra-stable mineralization of beryllium in lithium slag is briefly described as follows: prepare 10% sodium phosphate solution, sodium fluoride solution, calcium hydroxide solution or suspension respectively, add 50% water by mass to lithium slag for slurrying, add 3% sodium phosphate (the percentage of sodium phosphate relative to the dry weight of lithium slag) and 1% sodium fluoride (the percentage of sodium fluoride relative to the dry weight of lithium slag) by mass to the slurry lithium slag, stir mechanically for 30 minutes, then add 1% calcium hydroxide (the percentage of calcium hydroxide relative to the dry weight of lithium slag), stir mechanically for another 30 minutes, and the stabilization reaction is completed. After filtering and washing the stabilized lithium slag, the leaching toxicity of the treated lithium slag is tested, and the beryllium content in multiple batches of leachate is 0.005-0.014 mg / L, which is lower than the national standard.
[0037] The following table shows the treatment effect of beryllium ultra-stable mineralizing reagent composed of different amounts of sodium phosphate, sodium fluoride and calcium hydroxide on lithium slag (refer to Example 3 for specific operation):
[0038]
Claims
1. An ultrastable mineralization reagent for dangerous beryllium elements in lithium slag, characterized in that: Contains the following components by mass: Phosphate 1-5 parts; 1-2 parts of calcium compound; 1~2 parts of fluoride; The phosphate includes at least one of sodium phosphate and potassium phosphate; The calcium compound includes at least one of calcium carbonate, calcium hydroxide and calcium oxide; The fluoride includes at least one of calcium fluoride, sodium fluoride, potassium fluoride and hydrofluoric acid.
2. A method for ultrastable mineralization of dangerous beryllium elements in lithium slag, characterized in that: The ultra-stable beryllium mineralization reagent according to claim 1 is slurried, and then added to the slurried lithium slag or lithium mineral leaching slurry to carry out a mineralization reaction. After the mineralization reaction is completed, it is filtered and separated to obtain an ultra-stable mineralized lithium slag; The phosphate and fluoride are mixed and slurried, and then added to the slurried lithium slag or lithium mineral leaching slurry, and stirred for mineralization reaction; the calcium compound is then slurried, and then added to the slurried lithium slag or lithium mineral leaching slurry to continue the mineralization reaction; wherein the mass ratio of the phosphate, the fluoride and the calcium compound is (1-5):(1-2):(1-2), the total mass of the phosphate, the fluoride and the calcium compound is 1.0%-8.0% of the mass of the lithium slag in the slurried lithium slag or lithium mineral leaching slurry, and the mass of water in the slurried lithium slag accounts for 40%-200% of the mass of the lithium slag.
3. The method for ultrastable mineralization of dangerous beryllium elements in lithium slag according to claim 2, characterized in that: The temperature of the mineralization reaction is room temperature, and the total time is 20 to 60 minutes.