Mat material, exhaust gas purification device and mat material manufacturing method

By adding inorganic and organic binders to the surface of the inorganic fibers of the mat material, a high initial compression surface pressure is formed, which solves the problem of insufficient compression surface pressure of the mat material and ensures the sealing and stability of the exhaust gas purification device.

CN116997704BActive Publication Date: 2024-10-11IBIDEN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280021734.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-03-31
Filing Date
2022-03-23
Publication Date
2024-10-11
Estimated Expiration
2042-03-23

AI Technical Summary

Technical Problem

The initial compression surface pressure of the existing mat material is not high enough, causing the exhaust gas treatment body to be easily damaged when it comes into contact with the outer shell, and the problem of exhaust gas leakage is difficult to solve.

Method used

By adding inorganic binders and organic binders to the surface of inorganic fibers, the friction coefficient and sliding properties between fibers are increased, a concave-convex structure is formed, the initial compression surface pressure is increased, and the accumulation specific gravity and density of the fiber dispersion are controlled during the manufacturing process. The presence ratio of twist ensures a sufficient number of fiber joints.

Benefits of technology

The initial compression surface pressure of the mat material reaches more than 900kPa, preventing exhaust gas leakage and the treatment body from falling off. The compression surface pressure is not easily reduced under long-term stress application, making it suitable for use in exhaust gas purification devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116997704B_ABST
    Figure CN116997704B_ABST
Patent Text Reader

Abstract

The present invention provides a mat material with a sufficiently high initial compression surface pressure. The mat material of the present invention is a mat material in which an inorganic binder and an organic binder are added and attached to inorganic fibers, and is characterized in that the above-mentioned mat material is compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 900 kPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a mat material, an exhaust gas purification device and a method for manufacturing the mat material. Background Art

[0002] Exhaust gas from internal combustion engines such as diesel engines contains particulate matter such as soot (hereinafter also referred to as PM), and the harm caused by PM to the environment and human body has become a problem in recent years. In addition, exhaust gas also contains harmful gas components such as CO, HC, and NOx, so the impact of these harmful gas components on the environment and human body is also worrying.

[0003] Therefore, as an exhaust gas purification device for capturing PM in exhaust gas and purifying harmful gas components, various schemes of exhaust gas purification devices consisting of an exhaust gas treatment body (which is composed of porous ceramics), a shell that accommodates the exhaust gas treatment body, and a mat material (which is arranged between the exhaust gas treatment body and the shell and is composed of an inorganic fiber aggregate) have been proposed. The main purpose of arranging the mat material is to prevent the exhaust gas treatment body from contacting with the shell covering its outer periphery and being damaged due to vibration or impact caused by the driving of the car, etc.; to prevent exhaust gas from leaking from between the exhaust gas treatment body and the shell, etc. Therefore, the mat material is required to have the function of increasing the surface pressure generated by the rebound force caused by compression and reliably holding the exhaust gas treatment body.

[0004] As such a mat material, Patent Document 1 discloses a sealing material for a catalytic converter for automobile exhaust gas purification, characterized in that it is composed of a sheet-shaped molded body formed by integrating inorganic short fibers and an organic binder by a papermaking method, and the molded body expands 1.3 to 6 times in the thickness direction due to the burnout of the organic binder, generating a restoring surface pressure caused by the inorganic short fibers, and the molded body has a thickness of 100 cm2. 2 The fiber mass per unit plane area in any part is within ±8% of the mass average value.

[0005] In addition, Patent Document 1 discloses a method for manufacturing the sealing material, which is characterized in that inorganic short fibers are dispersed in a medium to prepare a slurry, and the sheet is formed into a desired shape by a papermaking method and then dried. When the slurry is cut as needed, an organic binder is present in the slurry, or is added after the sheet is formed, or both methods are used, and drying is carried out while applying a compressive force.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2003-262116 Summary of the invention

[0009] Problems to be solved by the invention

[0010] Patent Document 1 describes a method for producing a mat material by a papermaking method, but the obtained mat material has a problem that the initial compression surface pressure is not high enough.

[0011] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a mat material having a sufficiently high initial compression surface pressure.

[0012] Means for solving problems

[0013] The present inventors have repeatedly conducted intensive studies and have found that the reason why the initial compression surface pressure of the mat material of Patent Document 1 is low is that a large amount of twists formed by inorganic fibers twisted together are present in the inorganic fiber dispersion in which inorganic fibers are dispersed when the mat material is manufactured.

[0014] The mat material of the present invention is a mat material in which an inorganic binder and an organic binder are added and attached to inorganic fibers, and is characterized in that the mat material is compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 900 kPa or more.

[0015] In the mat material of the present invention, an inorganic binder is added and attached to the inorganic fiber. The inorganic binder forms concavities and convexities on the surface of the inorganic fiber. Such concavities and convexities increase the friction coefficient between the inorganic fibers. As a result, the initial compression surface pressure of the mat material is also increased.

[0016] In the mat material of the present invention, an organic binder is added and attached to the inorganic fibers. The organic binder makes it easy for the inorganic fibers to slide against each other, so that when a strong stress is applied to the inorganic fibers, the inorganic fibers can be offset and the inorganic fibers are not easily damaged. As a result, even when stress is continuously applied to the mat material, the compressive surface pressure of the mat material is not easy to reduce.

[0017] In the mat material of the present invention, the mat material is compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 900 kPa or more, and thus the initial compression surface pressure was sufficiently high.

[0018] Therefore, when the mat material of the present invention is used in an exhaust gas purification device, it is possible to prevent leakage of exhaust gas and prevent the exhaust gas treating body from falling off from the metal casing due to gas pressure.

[0019] In the mat material of the present invention, the weight ratio of the inorganic binder to the mat material is preferably greater than 0 wt % and not more than 10 wt %.

[0020] When the weight ratio of the inorganic binder contained in the mat of the present invention is within the above range, the number of concavities and convexities formed on the surface of the inorganic fibers is sufficiently increased, and the friction coefficient between the inorganic fibers is increased. As a result, the initial compression surface pressure of the mat is also increased.

[0021] In the mat material of the present invention, the weight ratio of the organic binder to the mat material is preferably greater than 0 wt % and less than 10 wt %.

[0022] When the weight ratio of the organic binder contained in the mat material of the present invention is within the above range, the inorganic fibers are easy to slide fully with each other and the inorganic fibers are not easy to be damaged. Therefore, even when stress is continuously applied to the mat material, the compression surface pressure of the mat material is not easy to reduce.

[0023] In the mat material of the present invention, it is preferred that the inorganic binder and the organic binder are added and attached to the surface of the inorganic fibers in a dispersed state.

[0024] When the inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber in a dispersed state, the inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber uniformly. Therefore, the effect of increasing the initial compression surface pressure of the mat material brought about by the inclusion of the inorganic binder and the organic binder, and the effect that the compression surface pressure of the mat material is not easily reduced even when stress is continuously applied to the mat material are improved.

[0025] The mat material of the present invention preferably further contains a polymer-based dispersant.

[0026] When the mat material of the present invention is produced, when the inorganic binder and the organic binder are added and attached to the surface of the inorganic fibers, if a polymer dispersant is used, the inorganic binder and the organic binder can be easily and uniformly added and attached to the surface of the inorganic fibers.

[0027] In the mat material of the present invention, an aggregate composed of the inorganic binder and the organic binder may be added and attached to the surface of the inorganic fiber.

[0028] Even if the aggregate composed of inorganic binder and organic binder is added and attached to the surface of inorganic fiber, the initial compression surface pressure of the mat can be improved, and the compression surface pressure of the mat is not easily reduced even when stress is continuously applied to the mat.

[0029] The mat material of the present invention may be a paper-made mat.

[0030] Paper-made mats are manufactured by papermaking inorganic fibers, so the inorganic fibers are not easily damaged during the manufacturing process. Therefore, it is easy to increase the initial compression surface pressure of the mat material.

[0031] The mat material of the present invention is preferably made by papermaking an inorganic fiber-binder mixed solution, wherein the inorganic fiber-binder mixed solution is an inorganic fiber dispersion having an inorganic fiber bulk specific gravity in water of 0.001 to 0.02 g / cm 3 The inorganic fiber dispersion is mixed with an inorganic binder and an organic binder.

[0032] The reason why the mat material generates surface pressure is that friction occurs at the contact points between inorganic fibers, thereby generating a force that hinders the movement of inorganic fibers. In the mat material, if the number of contact points between inorganic fibers is large, the number of places where friction occurs increases, so the surface pressure of the mat material increases.

[0033] When there is a twist formed by twisting inorganic fibers together in the mat material, the twisted inorganic fibers are bundled, so the twist can be regarded as one inorganic fiber. Therefore, the number of inorganic fibers in the mat material is reduced. In addition, the overall specific surface area of ​​the inorganic fibers contained in the mat material is reduced. In this way, the number of contact points between the inorganic fibers in the mat material is reduced, and the initial compression surface pressure of the mat material tends to decrease.

[0034] Bulk density in water is 0.001~0.02g / cm 3 In the inorganic fiber dispersion, the proportion of twists formed by the inorganic fibers twisting each other is reduced. In addition, in the mat material manufactured using such an inorganic fiber dispersion, the proportion of twists is also reduced. Therefore, the number of contact points between the inorganic fibers in the mat material can be made sufficient, and as a result, the initial compression surface pressure of the mat material is also increased.

[0035] In addition, in the mat material manufactured using such inorganic fiber dispersion, since the inorganic fibers are uniformly dispersed, it is easy to disperse stress. Therefore, even when stress is continuously applied to the mat material, the inorganic fibers are not easy to break. As a result, the compression surface pressure of the mat material is not easy to reduce even when stress is continuously applied to the mat material.

[0036] In the mat of the present invention, it is preferred that: the mat includes a twist formed by twisting the inorganic fibers together, and in a cross section parallel to the thickness direction of the mat, the ratio of the cross-sectional area of ​​the twist to the cross-sectional area of ​​the mat is greater than 0.5% and less than 10%.

[0037] When the ratio of the cross-sectional area of ​​the twist to the cross-sectional area of ​​the mat material is within the above range, the existence ratio of the twist becomes an appropriate ratio, and thus the initial compression surface pressure of the mat material increases.

[0038] In the mat material of the present invention, it is preferred that the mat material is compressed to a bulk density of 0.50 g / cm 3 , then released to a bulk density of 0.45g / cm 3When this operation is regarded as one cycle, after 1000 cycles, the bulk density is compressed to 0.45 g / cm 3 The compression surface pressure of the above-mentioned mat material is greater than 175 kPa.

[0039] Such a mat material is not easily degraded by the compressive surface pressure and is therefore suitable as a mat material for an exhaust gas purifying device.

[0040] The exhaust gas purification device of the present invention is an exhaust gas purification device comprising: an exhaust gas treatment body; a metal shell that accommodates the above-mentioned exhaust gas treatment body; and a mat material arranged between the above-mentioned exhaust gas treatment body and the above-mentioned metal shell to hold the above-mentioned exhaust gas treatment body, characterized in that the above-mentioned mat material is the above-mentioned mat material of the present invention.

[0041] The exhaust gas purification device of the present invention includes the above-mentioned mat of the present invention. Therefore, the initial compression surface pressure of the mat is sufficiently high to prevent leakage of exhaust gas and prevent the exhaust gas treatment body from falling off the metal casing due to gas pressure.

[0042] The manufacturing method of the mat material of the present invention is characterized in that it includes the following steps: a defibration step, in which water is added to the inorganic fibers before defibration to defibrate the inorganic fibers before defibration to prepare an inorganic fiber dispersion; an inorganic fiber-binder mixed liquid preparation step, in which the inorganic fiber dispersion is mixed with an inorganic binder and an organic binder to prepare an inorganic fiber-binder mixed liquid; a papermaking step, in which the inorganic fiber-binder mixed liquid is papermade and dehydrated to prepare a mat precursor; and a heating and pressurizing step, in which the mat precursor is heated and pressurized to prepare a mat material.

[0043] In the method for producing a mat material of the present invention, in the defibration step, the bulk density of the inorganic fibers in water after defibration reaches 0.001 to 0.02 g / cm 3 The above-mentioned inorganic fibers before defibration are defibrated in a manner.

[0044] By setting the bulk specific gravity in water of the defibrated inorganic fibers to be within the above range, the proportion of twist in the inorganic fiber dispersion can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 It is a perspective view schematically showing an example of the mat material of the present invention.

[0046] Figure 2 It is a cross-sectional view schematically showing an example of the exhaust gas purification device of the present invention.

[0047] Figure 3A It is a perspective view schematically showing an example of an exhaust gas treating body constituting the exhaust gas purifying device of the present invention.

[0048] Figure 3B yes Figure 3A AA line section view.

[0049] Figure 4 This is a cross-sectional photograph of a cross section of the mat material of Example 1 parallel to the thickness direction. DETAILED DESCRIPTION

[0050] The mat material of the present invention is described below.

[0051] However, the present invention is not limited to the following configurations, and can be applied with appropriate changes within the scope of the present invention. It should be noted that a configuration in which two or more of the preferred configurations of the present invention described below are combined also belongs to the present invention.

[0052] The mat material of the present invention will be described using the drawings.

[0053] Figure 1 It is a perspective view schematically showing an example of the mat material of the present invention.

[0054] like Figure 1 As shown, the mat 10 is rectangular in a plan view, and has a convex portion 11 a at one end 11 and a concave portion 12 a at the other end 12 so that the ends fit together when the mat 10 is wound around an object.

[0055] If such convex portions 11 a and concave portions 12 a are provided, the sealing performance is improved when the mat 10 is disposed in an exhaust gas purifying device described later.

[0056] It should be noted that Figure 1 In the mat material 10 shown, the convex portion 11a and the concave portion 12a are formed at the center of the short side direction of the mat material 10, but in the mat material of the present invention, the convex portion and the concave portion may not be formed at the center of the short side direction of the mat material as long as they can fit each other. For example, the side surface of the convex portion may be integrated with the side surface of the mat material. That is, when the mat material is viewed from above, the end portion may be formed in an L shape.

[0057] In addition, Figure 1 In the mat material 10 shown, the convex portion 11a and the concave portion 12a are rectangular, but in the mat material of the present invention, the convex portion and the concave portion may be in other shapes such as triangle, semicircle, etc. as long as they can fit each other.

[0058] In addition, Figure 1 In the mat material 10 shown, the convex portion 11 a and the concave portion 12 a are formed, but the mat material of the present invention may not have the convex portion and the concave portion at the end portion of the mat material.

[0059] As such a shape, for example, a parallelogram shape can be cited when the mat material is viewed from above. It should be noted that a parallelogram includes a rectangle. When the mat material is in such a shape, when the mat material is wound on an object, one end can be in contact with the other end. In addition, one end and the other end of the mat material do not need to be formed into a straight line, for example, a zigzag shape can be formed in which one end is in contact with the other end.

[0060] The mat material 10 is a mat material in which an inorganic binder and an organic binder are added and attached to inorganic fibers. The mat material 10 is compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 900 kPa or more.

[0061] The initial compression surface pressure is preferably 950 kPa or more, more preferably 1000 kPa or more. The initial compression surface pressure is preferably 1400 kPa or less, more preferably 1200 kPa or less.

[0062] In the mat material 10, an inorganic binder is added and attached to the inorganic fibers. The inorganic binder forms irregularities on the surface of the inorganic fibers. Such irregularities increase the friction coefficient between the inorganic fibers. As a result, the initial compression surface pressure of the mat material 10 is also increased.

[0063] In the mat material 10, an organic binder is added and attached to the inorganic fibers. The organic binder makes it easy for the inorganic fibers to slide against each other, so when a strong stress is applied to the inorganic fibers, the inorganic fibers can be offset and the inorganic fibers are not easily damaged. As a result, even when stress is continuously applied to the mat material 10, the compressive surface pressure of the mat material 10 is not easy to reduce.

[0064] The mat material 10 is compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 900 kPa or more, and thus the initial compression surface pressure was sufficiently high.

[0065] Therefore, when the mat 10 is used in an exhaust gas purifying device described later, it is possible to prevent leakage of exhaust gas and prevent the exhaust gas treating body from falling off from the metal casing due to gas pressure.

[0066] The surface pressure of the mat 10 can be measured using, for example, a hot surface pressure measuring device manufactured by MTS Corporation and equipped with a heater.

[0067] In addition, the mat material 10 is compressed to a bulk density of 0.50 g / cm 3 , then released to a bulk density of 0.45g / cm 3 When this operation is regarded as one cycle, after 1000 cycles, the bulk density is compressed to 0.45 g / cm 3The compressive surface pressure of the mat material 10 at the time of 175 kPa or more is preferably 175 to 230 kPa.

[0068] Such a mat 10 is not easily degraded by the compressive surface pressure and is therefore suitable as a mat for an exhaust gas purifying device described later.

[0069] That is, in the exhaust gas purifying device, exhaust gas repeatedly flows in. Therefore, the exhaust gas treating body and the metal casing constituting the exhaust gas purifying device repeatedly undergo volume changes due to heat.

[0070] As the volume of the exhaust gas treatment body and the metal shell changes, the mat material arranged in the exhaust gas purification device is repeatedly compressed and released.

[0071] When the mat 10 has the above-mentioned characteristics, the compression surface pressure of the mat 10 is sufficiently high even if it is repeatedly compressed and released, so that even if the exhaust gas repeatedly flows into the exhaust gas purification device, the exhaust gas treatment body can be fully held in the metal casing.

[0072] It should be noted that, in this specification, the above-mentioned one cycle means the following.

[0073] First, a mat material is placed between an upper plate and a lower plate of a hot surface pressure measuring device equipped with a heater.

[0074] Next, at room temperature, the upper plate was moved at a speed of 25.4 mm / min to compress the mat material to a bulk density of 0.50 g / cm 3 Keep it for 10 minutes.

[0075] Thereafter, while the mat was compressed, the upper plate was heated to 900°C at a heating rate of 45°C / min, and the lower plate was heated to 650°C.

[0076] Next, the upper plate was moved at a speed of 25.4 mm / min while the upper plate was kept at 900°C and the lower plate was kept at 650°C, and the mat was released to a bulk density of 0.45 g / cm 3 , and keep it in this state for 5 minutes. This compression and release is a preparatory operation for adapting the mat material to the device and is not included in the 1 cycle in the instructions.

[0077] Next, the upper plate was moved at a speed of 25.4 mm / min while the upper plate was kept at 900°C and the lower plate was kept at 650°C, and the mat was further compressed to a bulk density of 0.50 g / cm 3 , hold for 10 minutes.

[0078] Next, the upper plate was moved at a speed of 25.4 mm / min while the upper plate was kept at 900°C and the lower plate was kept at 650°C, and the mat was released again until the bulk density reached 0.45 g / cm 3 , hold for 10 minutes.

[0079] The mat material is compressed again to a bulk density of 0.50 g / cm 3 The process of releasing the mat material to a bulk density of 0.45g / cm 3 The process is 1 cycle.

[0080] The average fiber length of the inorganic fibers is preferably 0.1 to 10 mm, more preferably 0.2 to 8 mm.

[0081] If the average fiber length of the inorganic fibers is less than 0.1 mm, the fiber length of the inorganic fibers is too short, so the shape retention of the mat material is reduced. In addition, when the mat material is made, the inorganic fibers are not properly entangled with each other, and it is difficult to obtain sufficient surface pressure.

[0082] If the average fiber length of the inorganic fibers is greater than 10 mm, the fiber length of the inorganic fibers is too long. Therefore, in the papermaking process, in the inorganic fiber dispersion formed by dispersing the inorganic fibers in water, the entanglement between the inorganic fibers becomes too strong. Therefore, when the mat material is made, the inorganic fibers are prone to uneven aggregation and the shear strength is also prone to decrease.

[0083] Regarding the measurement of the inorganic fiber length, the inorganic fibers were extracted from the mat material using tweezers so as not to break, and the fiber length was measured using an optical microscope.

[0084] In this specification, the average fiber length refers to the average length obtained by extracting 300 inorganic fibers from the mat material and measuring the fiber length. In the case where the inorganic fibers cannot be extracted from the mat material in a manner that does not break, the mat material can be degreased and the degreased mat material can be put into water to untangle the inorganic fibers from each other while collecting the inorganic fibers in a manner that does not break.

[0085] In the mat 10 , the average fiber diameter of the inorganic fibers is preferably 3 to 8 μm, more preferably 5 to 7 μm.

[0086] If the average fiber diameter of the inorganic fibers is less than 3 μm, the strength of the inorganic fibers is weak and the inorganic fibers are easily cut by impact or the like.

[0087] If the average fiber diameter of the inorganic fibers is larger than 8 μm, the fiber diameter is too thick, the Young's modulus of the inorganic fibers themselves increases, and the flexibility of the mat material tends to decrease.

[0088] Examples of the inorganic fibers include alumina fibers, alumina-silica fibers, silica fibers, glass wool, and rock wool. Among these, alumina-silica fibers are preferred.

[0089] These inorganic fibers have high heat resistance, and a mat material formed of such inorganic fibers is unlikely to change shape due to temperature changes.

[0090] In addition, when the inorganic fiber is alumina-silica fiber, the composition ratio of alumina to silica is preferably alumina (Al2O3):silica (SiO2) = 60:40 to 80:20 in weight ratio, and more preferably alumina (Al2O3):silica (SiO2) = 70:30 to 74:26.

[0091] In the mat material 10, two or more kinds of inorganic fibers may be used in combination.

[0092] In the mat material 10 , the type of the inorganic binder is not particularly limited, and alumina sol, silica sol, aerogel, fumed silica, titanium particles, etc. can be used.

[0093] In the mat material 10 , two or more inorganic binders may be used in combination.

[0094] In the mat material 10, the weight ratio of the inorganic binder to the mat material 10 is preferably greater than 0 wt%, more preferably 0.3 wt% or more. In addition, the weight ratio is preferably 10 wt% or less, more preferably 8 wt% or less.

[0095] When the weight ratio of the inorganic binder contained in the mat 10 is within the above range, the number of irregularities formed on the surface of the inorganic fibers is sufficiently increased, and the friction coefficient between the inorganic fibers is increased. As a result, the initial compression surface pressure of the mat is also increased.

[0096] In the mat 10 , the type of the organic binder is not particularly limited, and rubber-based resins, styrene-based resins, silicone-based resins, acrylic-based resins, polyester-based resins, polyurethane resins, and the like can be used.

[0097] In the mat material 10 , two or more kinds of organic binders may be used in combination.

[0098] In the mat material 10, the weight ratio of the organic binder to the mat material 10 is preferably greater than 0 wt%, more preferably 0.3 wt% or more. In addition, the weight ratio is preferably 10 wt% or less, more preferably 8 wt% or less.

[0099] When the weight ratio of the organic binder contained in the mat material 10 is within the above range, the inorganic fibers can easily slide sufficiently with each other and the inorganic fibers are not easily damaged. Therefore, even when stress is continuously applied to the mat material 10, the compressive surface pressure of the mat material 10 is not easily reduced.

[0100] The mat material 10 may contain a polymer dispersant, a coagulant, and a surfactant in addition to the organic binder and the inorganic binder.

[0101] When the inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber in the case of manufacturing the mat material 10, if a polymer dispersant is used, the inorganic binder and the organic binder are easily and uniformly added and attached to the surface of the inorganic fiber. Therefore, the effect of increasing the initial compression surface pressure of the mat material 10 and the effect of not easily reducing the compression surface pressure of the mat material 10 even when stress is continuously applied to the mat material 10 are improved.

[0102] Furthermore, the mat material 10 manufactured in this manner contains a polymer-based dispersant.

[0103] The polymer dispersant is not particularly limited, and examples thereof include anionic polymer dispersants such as polycarboxylic acids and / or their salts, naphthalenesulfonate formaldehyde condensates and / or their salts, polyacrylic acid and / or their salts, polymethacrylic acid and / or their salts, polyvinylsulfonic acid and / or their salts, and hydrophilic synthetic polymer substances such as nonionic polymer dispersants such as polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene glycol; natural hydrophilic polymer substances such as gelatin, casein, and water-soluble starch; hydrophilic semi-synthetic polymer substances such as carboxymethyl cellulose; and the like.

[0104] Among these, hydrophilic synthetic polymer substances are preferred, and anionic polymer dispersants are more preferred. The number average molecular weight of the anionic polymer dispersant is preferably 500 to 100000. The number average molecular weight of the anionic polymer dispersant can be calculated, for example, by molecular weight measurement based on gel permeation chromatography (GPC).

[0105] The coagulant is not particularly limited, and examples thereof include acrylamide and the like.

[0106] When a coagulant is used in manufacturing the mat 10 , the inorganic binder and the organic binder are easily entangled with the inorganic fibers.

[0107] In addition, the thickness of the mat material 10 is preferably 5 to 20 mm.

[0108] If the thickness of the mat material is less than 5 mm, the surface pressure of the mat material is likely to decrease. In addition, when the mat material is used in the exhaust gas purification device described later, the exhaust gas treatment body is likely to fall off. In addition, when the exhaust gas treatment body undergoes a volume change, the mat material is not likely to absorb the volume change of the exhaust gas treatment body. Therefore, cracks, etc., are likely to occur in the exhaust gas treatment body.

[0109] If the thickness of the mat material exceeds 20 mm, it loses its flexibility and becomes difficult to handle. In addition, when the mat material is wound around the exhaust gas treatment body described later, it is easy to generate winding wrinkles and cracks.

[0110] The basis weight (weight per unit area) of the mat material 10 is not particularly limited, but is preferably 200 to 4000 g / m 2 , more preferably 900 to 3000 g / m 2 .

[0111] If the base weight of the mat is less than 200g / m 2 , then the holding force is not easy to become sufficient.

[0112] If the base weight of the mat material is greater than 4000g / m 2 , the volume of the cushion material is not easy to reduce.

[0113] The bulk density of the mat material 10 when not compressed is preferably 0.10 to 0.30 g / cm 3 , more preferably 0.10 to 0.25 g / cm 3 .

[0114] If the bulk density of the mat material is less than 0.10g / cm 3 , the entanglement of the inorganic fibers is weak and the inorganic fibers are easily peeled off, so it is difficult to maintain the shape of the mat in a predetermined shape.

[0115] If the bulk density of the mat material is greater than 0.30g / cm 3 , the mat material becomes hard, so the mat material is easy to break.

[0116] In the mat material 10 , it is preferred that the inorganic binder and the organic binder are added and attached to the surface of the inorganic fibers in a dispersed state.

[0117] When the inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber in a dispersed state, the inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber uniformly. Therefore, the effect of increasing the initial compression surface pressure of the mat material 10 brought about by the inclusion of the inorganic binder and the organic binder, and the effect that the compression surface pressure of the mat material 10 is not easily reduced even when stress is continuously applied to the mat material 10 are improved.

[0118] It should be noted that, in the mat material 10 , aggregates composed of an inorganic binder and an organic binder may be added and attached to the surface of the inorganic fibers.

[0119] Even if the surface of the inorganic fiber is added with agglomerates composed of inorganic binders and organic binders, the initial compression surface pressure of the mat 10 can be improved, and the compression surface pressure of the mat 10 is not easily reduced even when stress is continuously applied to the mat 10.

[0120] In the mat material 10, whether the inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber in a dispersed state respectively, or whether the agglomerates composed of the inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber can be determined by removing the inorganic fiber from the mat material 10 and observing the surface of the inorganic fiber using a scanning electron microscope (SEM).

[0121] The mat 10 may be a paper-made mat or a needle-punched mat, but is preferably a paper-made mat.

[0122] When the mat 10 is a paper-made mat, the mat 10 is manufactured by paper-making inorganic fibers, so the inorganic fibers are not easily damaged during the manufacturing process. Therefore, the initial compression surface pressure of the mat 10 can be easily increased.

[0123] In addition, simply by adding an inorganic binder and an organic binder to an inorganic fiber dispersion used in papermaking, the inorganic binder and the organic binder can be added and attached to the obtained inorganic fibers.

[0124] In addition, when the mat material 10 is a paper-made mat, the mat material 10 is preferably made by paper-making the following inorganic fiber-binder mixed solution, wherein the inorganic fiber-binder mixed solution is an inorganic fiber dispersion liquid containing inorganic fibers having a bulk specific gravity in water of 0.001 to 0.02 g / cm 3 The inorganic fiber dispersion is mixed with an inorganic binder and an organic binder. It should be noted that the bulk density of the inorganic fibers in the inorganic fiber dispersion is more preferably 0.002 to 0.01 g / cm 3 .

[0125] The reason why the mat 10 generates surface pressure is that friction occurs at the contact points between inorganic fibers, thereby generating a force that hinders the movement of inorganic fibers. In the mat 10, if the number of contact points between inorganic fibers is large, the number of places where friction occurs increases, so the surface pressure of the mat 10 increases.

[0126] If there is a twist formed by twisting inorganic fibers with each other in the mat material 10, the twisted inorganic fibers are bundled, so the twist can be regarded as one inorganic fiber. Therefore, the number of inorganic fibers in the mat material 10 is reduced. In addition, the overall specific surface area of ​​the inorganic fibers contained in the mat material 10 is reduced. In this way, the number of contact points between the inorganic fibers in the mat material 10 is reduced, and the initial compression surface pressure of the mat material 10 tends to decrease.

[0127] Bulk density in water is 0.001~0.02g / cm 3In the inorganic fiber dispersion, the ratio of twists formed by twisting the inorganic fibers with each other is reduced. In addition, in the mat material 10 manufactured using such an inorganic fiber dispersion, the ratio of twists is also reduced. Therefore, the number of contact points between the inorganic fibers in the mat material 10 can be made sufficiently large, and as a result, the initial compression surface pressure of the mat material 10 is also improved.

[0128] In addition, in the mat material 10 manufactured using such inorganic fiber dispersion, the inorganic fibers are uniformly dispersed, so it is easy to disperse the stress. Therefore, even when the mat material 10 is continuously stressed, the inorganic fibers are not easily damaged. As a result, even when the mat material 10 is continuously stressed, the compression surface pressure of the mat material 10 is not easy to reduce.

[0129] In addition, in this specification, the bulk specific gravity in water of the inorganic fibers of the mat material refers to a value measured by the following method.

[0130] First, the mat material was heat treated at 600° C. for 1 hour to burn off the organic components.

[0131] Next, 0.5 g of inorganic fibers were collected from the heat-treated mat while being disassembled by hand. Thereafter, the collected inorganic fibers were placed in a container containing 80 mL of water and stirred at 1000 rpm for 10 minutes.

[0132] Next, the aqueous solution containing the inorganic fibers was transferred to a 100 mL measuring cylinder, and water was further added until the lower surface of the concave meniscus of the aqueous solution was located at the 100 mL mark.

[0133] After standing for 30 minutes, read the sedimentation height of the inorganic fibers, and take the product of the sedimentation height of the inorganic fibers and the bottom area of ​​the measuring cylinder as the volume of the inorganic fibers in water. Divide the weight of the inorganic fibers (0.5 g) by the volume of the inorganic fibers in water, and take the resulting value as the bulk density of the inorganic fibers in water of the mat.

[0134] The mat material 10 is preferably produced by papermaking an inorganic fiber-binder mixed solution obtained by mixing an inorganic fiber dispersion containing a surfactant, an inorganic binder, and an organic binder.

[0135] When preparing the inorganic fiber dispersion, water is added to the pre-fiberized inorganic fibers to break them into short fibers, thereby performing defibration. At this time, if defibration is performed in the presence of a surfactant, the obtained inorganic fibers are less likely to be twisted and twisted.

[0136] When the mat 10 is made of a twist-less inorganic fiber dispersion, the ratio of twist in the obtained mat 10 is also reduced, and the initial compression surface pressure of the mat 10 is increased. In addition, even when stress is continuously applied to the mat 10, the compression surface pressure of the mat 10 is not easy to reduce.

[0137] The type of surfactant is not particularly limited, and examples thereof include polycarboxylic acid-based surfactants and acrylic acid-based surfactants.

[0138] Among these, polycarboxylic acid-based surfactants are preferred. Polycarboxylic acid-based surfactants can increase the negative charge on the fiber surface, and the inorganic fibers repel each other, so that the inorganic fibers are less likely to be twisted together.

[0139] When the mat 10 is a paper-made mat, the mat 10 includes a twist formed by twisting inorganic fibers with each other, and in a cross section parallel to the thickness direction of the mat 10, the ratio of the cross-sectional area of ​​the twist to the cross-sectional area of ​​the mat 10 is preferably 0.5% or more, more preferably 0.7% or more. In addition, the cross-sectional area ratio of the twist is preferably 10% or less, more preferably 9% or less.

[0140] When the ratio of the cross-sectional area of ​​the twist to the cross-sectional area of ​​the mat 10 is within the above range, the existence ratio of the twist reaches an appropriate ratio, and thus the initial compression surface pressure of the mat 10 increases.

[0141] In addition, in this specification, the ratio of the cross-sectional area of ​​the twist to the cross-sectional area of ​​the mat material refers to a value calculated by the following method.

[0142] First, the mat material is cut parallel to the thickness direction, and the cut surface is scanned. Next, a range of 50 mm in length × width = 50 mm is selected at an arbitrary position of the cross section, and the range is acquired as image data.

[0143] The obtained image data is binarized so that a twisted cross-sectional portion and a non-twisted cross-sectional portion can be distinguished.

[0144] Next, the area of ​​the twisted cross section is calculated, and the ratio of the area of ​​the twisted cross section in the image is calculated.

[0145] The same operation was repeated three times except changing the selection range in the mat cross section, and the average value of the ratio of the twisted cross section area in each image was taken as the ratio of the twisted cross section area to the mat cross section area.

[0146] Next, an exhaust gas purification device using the mat material 10 will be described.

[0147] It should be noted that an exhaust gas purification device using the mat material 10 is also one embodiment of the present invention.

[0148] Figure 2 It is a cross-sectional view schematically showing an example of the exhaust gas purification device of the present invention.

[0149] like Figure 2 As shown, the exhaust gas purifying device 1 includes an exhaust gas treating body 20, a metal casing 30 accommodating the exhaust gas treating body 20, and a mat 10 disposed between the exhaust gas treating body 20 and the metal casing 30. In the exhaust gas purifying device 1, the mat 10 functions as a holding sealing material.

[0150] The exhaust gas purifying device 1 includes a mat 10. The mat 10 has a sufficiently high initial compression surface pressure, and thus can prevent leakage of exhaust gas and prevent the exhaust gas treating body 20 from falling off from the metal casing 30 due to gas pressure.

[0151] Next, the exhaust gas treating body 20 constituting the exhaust gas purifying device 1 will be described.

[0152] Figure 3A It is a perspective view schematically showing an example of an exhaust gas treating body constituting the exhaust gas purifying device of the present invention. Figure 3B yes Figure 3A AA line section view.

[0153] like Figure 3A and Figure 3B As shown, the exhaust gas treatment body 20 included in the exhaust gas purification device 1 is a cylindrical treatment body in which a plurality of channels 21 are arranged in parallel along the length direction with a channel wall 22 interposed therebetween.

[0154] The exhaust gas treating body 20 is an exhaust gas filter (honeycomb filter) in which any one of the cells 21 is sealed with a sealing material 23 .

[0155] like Figure 3B As shown, the exhaust gas ( Figure 3B , the exhaust gas is represented by G and the flow of the exhaust gas is represented by arrows) flows into a channel 21 opened on the exhaust gas inlet side end face of the exhaust gas treatment body 20, and passes through the channel wall 22 that separates the channel 21. At this time, PM in the exhaust gas is captured by the channel wall 22, and the exhaust gas is purified. The purified exhaust gas flows out from other channels 21 opened on the exhaust gas outflow side end face and is discharged to the outside.

[0156] It should be noted that Figure 3A and Figure 3B The exhaust gas treatment body 20 shown is a filter in which any end of the pores 21 is sealed by a sealing material 23, but in the exhaust gas treatment body constituting the exhaust gas purification device of the present invention, the ends of the pores may not be sealed. Such an exhaust gas treatment body can be suitably used as a catalyst carrier.

[0157] The exhaust gas treating body 20 may be made of non-oxidizing porous ceramics such as silicon carbide and silicon nitride, or may be made of oxidizing porous ceramics such as sialon, alumina, cordierite, and mullite. Among these, silicon carbide is preferred.

[0158] When the exhaust gas treating body 20 is a porous ceramic of silicon carbide, the porosity of the porous ceramic is not particularly limited, but is preferably 35 to 60%.

[0159] If the porosity is less than 35%, the exhaust gas treatment body may be immediately clogged. On the other hand, if the porosity is greater than 60%, the strength of the exhaust gas treatment body is reduced and the exhaust gas treatment body may be easily damaged.

[0160] In addition, the average pore diameter of the porous ceramic is preferably 5 to 30 μm.

[0161] If the average pore size is less than 5 μm, PM may easily cause clogging.

[0162] If the average pore size is larger than 30 μm, PM will pass through the pores and cannot be captured, which may result in the filter not being able to function as a filter.

[0163] In addition, the said porosity and pore diameter can be measured by the conventionally well-known method which measures using a scanning electron microscope (SEM).

[0164] The cell density at the cross section of the exhaust gas treatment body 20 is not particularly limited, but the preferred lower limit is 31.0 cells / cm 2 (200 pcs / inch 2 ), the preferred upper limit is 93.0 pcs / cm 2 (600 pcs / inch 2 ). In addition, the more preferred lower limit is 38.8 pieces / cm 2 (250pcs / inch 2 ), and the more preferred upper limit is 77.5 pieces / cm 2 (500 pcs / inch 2 ).

[0165] The exhaust gas treatment body 20 may be loaded with a catalyst for purifying the exhaust gas. As the loaded catalyst, for example, precious metals such as platinum, palladium, and rhodium are preferred, with platinum being more preferred. In addition, as other catalysts, alkali metals such as potassium and sodium, and alkaline earth metals such as barium may also be used. These catalysts may be used alone or in combination of two or more.

[0166] When loaded with these catalysts, PM can be easily burned and removed, and toxic exhaust gas can also be purified.

[0167] Next, the metal casing 30 constituting the exhaust gas purifying device 1 will be described.

[0168] The metal housing 30 has a substantially cylindrical shape.

[0169] The inner diameter of the metal casing 30 (the inner diameter of the portion that houses the exhaust gas treating body) is preferably slightly smaller than the diameter of the exhaust gas treating body 20 around which the mat 10 is wound.

[0170] When the inner diameter of the metal casing 30 is of such a length, after the exhaust gas treating body 20 wound with the mat 10 is pressed into the metal casing 30 , the mat 10 is compressed, and thus surface pressure is generated on the mat 10 .

[0171] As described above, since the initial compression surface pressure of the mat 10 is sufficiently high, it is possible to prevent the exhaust gas from leaking and prevent the exhaust gas treating body 20 from falling off from the metal casing 30 due to the gas pressure.

[0172] The metal case 30 is not particularly limited, but is preferably made of stainless steel.

[0173] Next, a method for producing the mat of the present invention will be described.

[0174] The manufacturing method of the mat material of the present invention includes the following steps: a defibration step, in which water is added to inorganic fibers before defibration to defibrate the inorganic fibers before defibration to prepare an inorganic fiber dispersion; an inorganic fiber-binder mixed liquid preparation step, in which the inorganic fiber dispersion is mixed with an inorganic binder and an organic binder to prepare an inorganic fiber-binder mixed liquid; a papermaking step, in which the inorganic fiber-binder mixed liquid is papermade and dehydrated to prepare a mat precursor; and a heating and pressurizing step, in which the mat precursor is heated and pressurized to prepare the mat material.

[0175] Each step is described in detail below.

[0176] [Fiberization process]

[0177] In the defibration step, water is added to inorganic fibers before defibration to defibrate the inorganic fibers before defibration to prepare an inorganic fiber dispersion.

[0178] The pre-fiberizing inorganic fibers may be produced by a conventionally known method or may be commercially available products.

[0179] As a method for producing inorganic fibers before defibration, for example, the following method can be mentioned.

[0180] That is, a spinning mixture containing basic aluminum chloride and silica sol is spun by a blow molding method to produce an inorganic fiber precursor, and then the inorganic fiber precursor is compressed to produce a rectangular sheet, and the compressed sheet is fired to produce pre-fiberized inorganic fibers composed of silica-alumina fibers.

[0181] The defibration method is not particularly limited, and the inorganic fibers before defibration may be dry defibrated and then wet defibrated by adding water, or wet defibration may be performed by adding water from the beginning.

[0182] Defiberization can be carried out using equipment such as a slush pulper, a feather mill, a disc mill, a bale opener, a pulper, a hammer mill, a carding machine, and a defibering machine.

[0183] The defibration may be performed using one type of equipment or two or more types of equipment.

[0184] When wet defibration is performed, it is preferred to use a pulp mill for defibration.

[0185] As a method of wet defibration using a pulp mill, for example, the following method can be mentioned.

[0186] The following method can be used: 1,000 L of water is added to 10 kg of pre-fibrillated inorganic fibers, and the mixture is stirred with a pulp mill at 2000 to 5000 rpm for 5 to 60 minutes to break the pre-fibrillated inorganic fibers into short fibers, thereby performing defibration.

[0187] In the defibration step, it is preferred that a surfactant is further added to the pre-defibration inorganic fibers to defibrate the pre-defibration inorganic fibers.

[0188] The presence of a surfactant during the defibration of the inorganic fibers before defibration can reduce entanglement between the inorganic fibers. As a result, the proportion of twists formed by the inorganic fibers being twisted together in the inorganic fiber dispersion after the defibration step is reduced.

[0189] By using such an inorganic fiber dispersion with a low twist ratio to carry out the inorganic fiber-binder mixture preparation process, papermaking process and heating and pressing process, a mat material with a sufficiently high initial compression surface pressure can be manufactured. In addition, the compression surface pressure of the mat material manufactured in this way is not easy to decrease even when stress is continuously applied.

[0190] The type of surfactant used in the defibration step is not particularly limited, and examples thereof include polycarboxylic acid-based surfactants and acrylic acid-based surfactants.

[0191] The amount of the surfactant used in the fibrillation step is not particularly limited, but is preferably 0.1 to 10 g per 1 L of water.

[0192] In the defibration step, it is preferred that the bulk specific gravity of the defibrated inorganic fibers in water be 0.001 to 0.02 g / cm 3The inorganic fibers before defibration are defibrated in a manner such that the bulk density in water is 0.002 to 0.01 g / cm 3 The inorganic fibers before defibration are defibrated in a manner.

[0193] By setting the bulk specific gravity in water of the defibrated inorganic fibers to be within the above range, the proportion of twist in the inorganic fiber dispersion can be reduced.

[0194] Furthermore, when a mat is produced by performing the steps described later using such an inorganic fiber dispersion, the ratio of twist contained in the produced mat is also reduced.

[0195] Therefore, the number of contact points between the inorganic fibers in the mat can be increased sufficiently, and as a result, the initial compression surface pressure of the mat is also increased.

[0196] In addition, in the mat material manufactured using such inorganic fiber dispersion, since the inorganic fibers are uniformly dispersed, stress is easily dispersed. Therefore, even when stress is continuously applied to the manufactured mat material, the inorganic fibers are not easily damaged. As a result, the compression surface pressure of the mat material is not easy to reduce even when stress is continuously applied to the manufactured mat material.

[0197] In addition, the bulk specific gravity in water of the defibrated inorganic fibers in this specification refers to a value measured by the following method.

[0198] First, the defibrated inorganic fibers were heat treated at 600° C. for 1 hour to dry them.

[0199] Next, 0.5 g of the heat-treated inorganic fibers were collected, and then the collected inorganic fibers were placed in a container containing 80 mL of water and stirred at 1000 rpm for 10 minutes.

[0200] Next, the aqueous solution containing the inorganic fibers was transferred to a 100 mL measuring cylinder, and water was further added until the lower surface of the concave meniscus of the aqueous solution was located at the 100 mL mark.

[0201] After standing for 30 minutes, read the sedimentation height of the inorganic fibers, and take the product of the sedimentation height of the inorganic fibers and the bottom area of ​​the measuring cylinder as the volume of the inorganic fibers in water. Divide the weight of the inorganic fibers (0.5 g) by the volume of the inorganic fibers in water, and take the resulting value as the bulk specific gravity of the defibrated inorganic fibers in water.

[0202] [Inorganic fiber-binder mixture preparation process]

[0203] In the inorganic fiber-binder mixed solution preparation step, the inorganic fiber dispersion prepared in the defibration step is mixed with an inorganic binder and an organic binder to prepare an inorganic fiber-binder mixed solution.

[0204] The type of the inorganic binder is not particularly limited, and alumina sol, silica sol, aerogel, fumed silica, titanium particles, etc. can be used.

[0205] The weight of the inorganic binder added is preferably greater than 0 wt%, more preferably greater than 0.3 wt%, relative to the weight of the inorganic fibers contained in the inorganic fiber dispersion, and preferably less than 10 wt%, more preferably less than 8 wt%.

[0206] The type of the organic binder is not particularly limited, and rubber-based resins, styrene-based resins, silicone-based resins, acrylic-based resins, polyester-based resins, polyurethane resins, and the like can be used.

[0207] The weight of the organic binder added is preferably greater than 0 wt%, more preferably greater than 0.3 wt%, relative to the weight of the inorganic fibers contained in the inorganic fiber dispersion, and preferably less than 10 wt%, more preferably less than 8 wt%.

[0208] It should be noted that in this step, a polymer dispersant, a coagulant, or a surfactant may be further added to the inorganic fiber dispersion.

[0209] When a polymer dispersant is added to the inorganic fiber dispersion, the inorganic binder and the organic binder are easily and evenly added and attached to the inorganic fiber surface. Therefore, the initial compression surface pressure of the mat material obtained through the steps described below is easily increased, and the compression surface pressure of the mat material is not easy to decrease even when stress is continuously applied to the mat material.

[0210] The polymer dispersant is not particularly limited, and examples thereof include anionic polymer dispersants such as polycarboxylic acids and / or their salts, naphthalenesulfonate formaldehyde condensates and / or their salts, polyacrylic acid and / or their salts, polymethacrylic acid and / or their salts, polyvinylsulfonic acid and / or their salts, and hydrophilic synthetic polymer substances such as nonionic polymer dispersants such as polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene glycol; natural hydrophilic polymer substances such as gelatin, casein, and water-soluble starch; hydrophilic semi-synthetic polymer substances such as carboxymethyl cellulose; and the like.

[0211] Among these, hydrophilic synthetic polymer substances are preferred, and anionic polymer dispersants are more preferred. The number average molecular weight of the anionic polymer dispersant is preferably 500 to 100,000.

[0212] The coagulant is not particularly limited, and examples thereof include acrylamide and the like.

[0213] When a coagulant is used, the inorganic binder and the organic binder are easily entangled with the inorganic fibers.

[0214] [Papermaking process]

[0215] In the papermaking step, the inorganic fiber-binder mixed solution prepared in the inorganic fiber-binder mixed solution preparing step is papermade and dehydrated to prepare a mat precursor.

[0216] The method and conditions for papermaking and dehydration are not particularly limited, and conventionally known methods and conditions can be used.

[0217] For example, it is preferred to use a continuous papermaking machine so that the basis weight of the mat material after production is 1000 to 3000 g / m 2 The method of copying is to

[0218] [Heating and Pressing Process]

[0219] In the heating and pressing step, the mat precursor produced in the papermaking step is heated and pressed to produce a mat material.

[0220] The conditions for heating and pressing are preferably 100 to 300° C. and 5 to 15 minutes.

[0221] Through the above steps, the mat material of the present invention can be manufactured.

[0222] Furthermore, the obtained mat material can be cut as needed to obtain a desired size.

[0223] (Example)

[0224] The following are examples that more specifically disclose the present invention. It should be noted that the present invention is not limited to these examples.

[0225] (Example 1)

[0226] [Fiberization process]

[0227] In an alkaline aluminum chloride aqueous solution prepared in such a manner that the Al content is 70 g / L and Al:Cl=1:1.8 (atomic ratio), silica sol is mixed in such a manner that the composition ratio of the fired inorganic fibers is Al2O3:SiO2=72:28 (weight ratio), and an appropriate amount of an organic polymer (polyvinyl alcohol) is further added to prepare a mixed solution.

[0228] The obtained mixed solution is concentrated to prepare a spinning mixture, and the spinning mixture is spun by a blowing method to prepare an inorganic fiber precursor. The inorganic fiber precursor is then compressed to prepare a rectangular sheet. The compressed sheet is fired at a maximum temperature of 1250°C to prepare an inorganic fiber before defibration containing 72 parts by weight of alumina and 28 parts by weight of silica.

[0229] 10 kg of the above-mentioned inorganic fibers before defibration are put into 1000 L of water, and a polycarboxylic acid surfactant (trade name: POISE 530, manufacturer: Kao Corporation) is further added as a surfactant at a concentration of 1 g / L. A commercially available blender (capacity of about 2000 L) is used to stir at 650 rpm for 20 minutes to break the inorganic fibers before defibration into short fibers, thereby defibring the inorganic fibers before defibration to prepare an inorganic fiber dispersion.

[0230] It should be noted that the bulk density of the inorganic fiber in water after defibration is 0.01 g / cm 3 .

[0231] [Inorganic fiber-binder mixture preparation process]

[0232] Next, AS200 (manufacturer: Nissan Chemical Co., Ltd.) as an inorganic binder and Nipool Lx854E (manufacturer: Nippon Zeon Co., Ltd.) as an organic binder were added to the inorganic fiber dispersion, and stirred at 650 rpm for 1 minute to prepare an inorganic fiber-binder mixed solution.

[0233] At this time, the weight of the inorganic binder is 2wt% relative to the weight of the inorganic fibers contained in the inorganic fiber dispersion, the weight of the organic binder is 7wt% relative to the weight of the inorganic fibers contained in the inorganic fiber dispersion, and the weight of the polymer dispersant is 1wt% relative to the weight of the inorganic fibers contained in the inorganic fiber dispersion.

[0234] [Papermaking process]

[0235] Next, the prepared inorganic fiber-binder mixed solution was made by a conventional method using a continuous papermaking machine so that the basis weight after drying was 1500 g / m 2 The mat precursor is made by papermaking.

[0236] [Heating and Pressing Process]

[0237] Next, the mat precursor was heated and pressed at 200° C. for 10 minutes using a press machine to prepare a mat material.

[0238] The mat of Example 1 was manufactured by cutting the mat material to 300 cm in the long side direction and 100 cm in the short side direction.

[0239] The mat material of Example 1 was compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 902 kPa.

[0240] The mat material of Example 1 was cut parallel to the thickness direction, and the cut surface was scanned. A cross-sectional photograph of the cross section of the mat material of Example 1 is shown in FIG. Figure 4 .

[0241] Figure 4 This is a cross-sectional photograph of a cross section of the mat material of Example 1 parallel to the thickness direction.

[0242] like Figure 4 As shown, it was observed that the mat material of Example 1 contained inorganic fibers twisted together ( Figure 4 Indicated by arrows).

[0243] The ratio of the cross-sectional area of ​​the twist to the cross-sectional area of ​​the mat of Example 1 was measured and found to be 0.5%.

[0244] (Comparative Example 1)

[0245] A mat of Comparative Example 1 was produced in the same manner as in Example 1 except that no inorganic binder was added in the inorganic fiber-binder mixed solution preparation step.

[0246] The mat material of Comparative Example 1 was compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 812 kPa.

[0247] (Comparative Example 2)

[0248] A mat material of Comparative Example 2 was produced in the same manner as in Example 1, except that no organic binder was added in the step of preparing the inorganic fiber-binder mixed solution.

[0249] The mat material of Comparative Example 2 was compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure was 885 kPa.

[0250] [Compression and release test]

[0251] The compressive surface pressure of the mats of Example 1 and Comparative Examples 1 and 2 after repeated compression and release was measured by the following method.

[0252] Each mat was placed between an upper plate and a lower plate of a hot surface pressure measuring device manufactured by MTS equipped with a heater.

[0253] Next, the upper plate was moved at a speed of 25.4 mm / min at room temperature to compress the mat material to a bulk density of 0.50 g / cm 3 Keep it for 10 minutes.

[0254] Thereafter, the upper plate was heated to 900° C. and the lower plate was heated to 650° C. at a heating rate of 45° C. / min while the mat was compressed.

[0255] Next, the upper plate was moved at a speed of 25.4 mm / min while the upper plate was kept at 900°C and the lower plate was kept at 650°C, and the mat was released to a bulk density of 0.45 g / cm 3 , and maintain this state for 5 minutes.

[0256] Next, the upper plate was moved at a speed of 25.4 mm / min while the upper plate was kept at 900°C and the lower plate was kept at 650°C, and the mat was further compressed to a bulk density of 0.50 g / cm 3 And keep it on for 10 minutes.

[0257] Next, the upper plate was moved at a speed of 25.4 mm / min while the upper plate was kept at 900°C and the lower plate was kept at 650°C, and the mat was released again until the bulk density reached 0.45 g / cm 3 , and keep it for 10 minutes.

[0258] Repeat 1000 cycles to compress the mat material to a bulk density of 0.50 g / cm 3 The process of releasing the mat material to a bulk density of 0.45g / cm 3 After 1000 cycles, the bulk density was 0.45 g / cm 3 The results are shown in Table 1.

[0259] [Table 1]

[0260] Example 1 Comparative Example 1 Comparative Example 2 Use of surfactants in the defibrination process use use use Inorganic binder Include Not included Include Organic binder Include Include Not included Initial compression surface pressure (kPa) 902 812 885 Compression surface pressure after compression and release test (kPa) 177 157 162

[0261] As shown in Table 1, it was found that when the mat material contained an inorganic binder and an organic binder, the initial compression surface pressure of the mat material was sufficiently increased, and the compression surface pressure after repeated compression and release was also sufficiently increased.

[0262] Explanation of symbols

[0263] 1. Exhaust gas purification device

[0264] 10. Mat

[0265] 11 One end

[0266] 11a convex part

[0267] 12 The other end

[0268] 12a recess

[0269] 20 Exhaust gas treatment body

[0270] 21 Channel

[0271] 22 Channel wall

[0272] 23 Sealing material

[0273] 30 Metal housing

Claims

1. A mat material, which is a mat material formed by adding an inorganic binder and an organic binder to inorganic fibers, characterized in that: The mat material is compressed to a bulk density of 0.50 g / cm 3 The measured initial compression surface pressure is 900 kPa or more. The mat material is a paper-made mat. The mat material is made by papermaking an inorganic fiber-binder mixed solution, wherein the inorganic fiber-binder mixed solution is an inorganic fiber dispersion liquid containing inorganic fibers having a bulk specific gravity in water of 0.001 g / cm 3 ~0.02g / cm 3 The inorganic fiber dispersion containing a surfactant is mixed with an inorganic binder and an organic binder. The mat material includes a twist formed by twisting the inorganic fibers with each other, and in a cross section parallel to a thickness direction of the mat material, a ratio of an area of ​​the cross section of the twist to an area of ​​a cross section of the mat material is 0.5% or more and 10% or less, The mat material contains the surfactant.

2. The mat material according to claim 1, wherein: The weight ratio of the inorganic binder to the mat material is greater than 0wt% and less than 10wt%.

3. The mat material according to claim 1 or 2, wherein: The weight ratio of the organic binder to the mat material is greater than 0 wt % and less than 10 wt %.

4. The mat material according to claim 1 or 2, wherein: The inorganic binder and the organic binder are added and attached to the surface of the inorganic fiber in a dispersed state.

5. The mat material according to claim 1 or 2, wherein: It further contains a polymer dispersant.

6. The mat material according to claim 1 or 2, wherein: Aggregates composed of the inorganic binder and the organic binder are added and attached to the surfaces of the inorganic fibers.

7. The mat material according to claim 1 or 2, wherein: The mat material is compressed to a bulk density of 0.50 g / cm 3 , then released to a bulk density of 0.45g / cm 3 When this operation is regarded as one cycle, after 1000 cycles, the bulk density is compressed to 0.45 g / cm 3 The compression surface pressure of the mat material is greater than 175 kPa.

8. A method for manufacturing a mat material, characterized in that: It includes the following steps: a defibration step of adding water and a surfactant to inorganic fibers before defibration to defibrate the inorganic fibers before defibration to prepare an inorganic fiber dispersion containing the surfactant; an inorganic fiber-binder mixed liquid preparation step, mixing the inorganic fiber dispersion liquid containing the surfactant with an inorganic binder and an organic binder to prepare an inorganic fiber-binder mixed liquid; A papermaking process, papermaking and dehydrating the inorganic fiber-binder mixed solution to form a mat precursor; as well as a heating and pressurizing step, heating and pressurizing the mat precursor to form a mat material; In the defibration step, the bulk density of the inorganic fibers in water after defibration reaches 0.001 g / cm 3 ~0.02g / cm 3 Defibrating the inorganic fiber before defibrating in a manner as follows, The inorganic fiber-binder mixture preparation process, the papermaking process and the heating and pressurizing process are carried out as follows: the mat material includes a twist formed by twisting the inorganic fibers with each other, and in a cross-section parallel to the thickness direction of the mat material, the ratio of the cross-sectional area of ​​the twist to the cross-sectional area of ​​the mat material is greater than 0.5% and less than 10%.