High carbon bearing steel for rolling element of main shaft bearing of wind turbine and production method thereof

Through vacuum degassing plus continuous casting process and chemical composition optimization, combined with rolling and spheroidizing annealing processes, the problems of high production cost and low efficiency of steel for wind turbine main shaft bearings are solved, and high performance, high efficiency and low cost are achieved. production effect.

CN117004881BActive Publication Date: 2024-10-11JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310441672.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-23
Publication Date
2024-10-11
Estimated Expiration
2043-04-23

AI Technical Summary

Technical Problem

The production cost of existing steel for main shaft bearings of wind turbines is high, and the efficiency of the electroslag remelting process is low, making it difficult to meet market competitiveness needs.

Method used

Vacuum degassing and continuous casting processes are used to produce high-carbon bearing steel. Through chemical composition optimization and process improvement, the content of elements such as C, Si, Mn, Cr, and Mo is designed, and the rolling and spheroidizing annealing processes are combined to improve the quenching of the steel. properties, toughness and wear resistance.

Benefits of technology

It reduces production costs, improves production efficiency and material quality stability, meets the high-performance requirements of wind turbine main shaft bearing rolling elements, and has strong market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117004881B_ABST
    Figure CN117004881B_ABST
Patent Text Reader

Abstract

The present invention relates to a high carbon bearing steel for a rolling element of a main shaft bearing of a wind turbine and a production method thereof, and belongs to the field of metallurgy. The mass percentage of the element components of the product is as follows: C: 0.90-1.05%, Si: 0.20-0.40%, Mn: 0.60-0.80%, Cr: 1.65-1.90%, Mo: 0.20-0.35%, Ni≤0.25%, Al≤0.05%, P≤0.010%, S: 0.005-0.015%, Cu≤0.20%, Ca≤0.0010%, Ti≤0.0015%, O≤0.0008%, and the remainder is Fe and unavoidable impurities. The metallographic structure of the surface layer of the steel after hot rolling is a troostite structure, and the core structure is a pearlite structure; the metallographic structure after spheroidizing annealing treatment is spheroidal carbide particles, and the spheroidization rate of the carbide particles on the cross section of the round steel is 100%. The production process of vacuum degassing and continuous casting is realized in the process, which improves the production efficiency, and adopts specific rolling and cooling processes to improve the carbide network of steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and more specifically relates to bearing steel and a corresponding production process. Background Art

[0002] Wind energy is currently the most promising renewable energy source. It is a clean, pollution-free green energy source. Among various alternative energy sources, wind energy has the broadest prospects for utilization and is increasingly valued by countries around the world. It has huge potential.

[0003] Wind turbine bearings are important transmission devices in wind turbines. A wind turbine can use up to 32 sets of bearings. Therefore, choosing the right bearings is very important to ensure the safe and stable operation of wind turbines. Wind turbine bearings are generally divided into the following types: yaw bearings, pitch bearings, main shaft bearings, speed increaser bearings and generator bearings. Different bearing types have different technical requirements.

[0004] Wind turbine bearings work in harsh conditions, with a wide range of temperature, humidity and load variations. Yaw and pitch bearings have to withstand large overturning moments, and main shaft and speed increaser bearings have to withstand large impact loads during startup and braking. Since wind turbines are required to start generating electricity when the wind speed reaches 3-4m / s, the bearings should have the characteristics of low friction torque and high operational flexibility. In addition, the most critical thing is that since hoisting and replacing bearings is extremely inconvenient and costly, the cost of installation and disassembly is as high as hundreds of thousands to millions. Therefore, a 20-year service life and high reliability have become the basic requirements for wind turbine bearings.

[0005] At present, the main players that dominate the global wind power bearing market are Sweden's SKF, Germany's FAG, the United States' TIMKEN and Japan's NSK. The production capacity of domestic wind power bearing companies is mainly concentrated in yaw bearings and pitch bearings with relatively low technical barriers. The supporting bearings for wind power equipment below 3MW can be mass-produced, and the domestic substitution rate has reached more than 80%, with an annual production capacity of more than 40,000 sets; while the main shaft bearings and speed increaser bearings have higher technical content and still rely on imports. Only some companies have initially intervened and are still in the research and development stage.

[0006] At present, the steel used for the main shaft bearings of domestic wind turbines is mainly bearing steel produced by the electroslag remelting process. The steel materials used include traditional high-carbon bearing steels GCr15 and GCr15SiMn, and carburized bearing steels such as G20Cr2Ni4 are also used. The steel produced by the electroslag remelting process has many quality advantages such as fine and uniform distribution of non-metallic inclusions, high uniformity of organization and high density. Therefore, its quality stability has always been good. However, the electroslag remelting production process also has obvious disadvantages such as very low production efficiency and production capacity, very high energy consumption and production costs. Therefore, the market competitiveness of electroslag remelting steel is very low. Patent No. CN109161658A is a kind of steel for the main shaft bearings of wind turbines and its production method. The patent proposes to use vacuum degassing and continuous casting process to produce steel for the main shaft bearings of wind turbines, and replace the electroslag process, so as to achieve the purpose of reducing costs. This patent involves carburized bearing steel, which can ensure sufficient hardness and wear resistance after carburizing treatment, and the core of the carburized bearing steel maintains the original metallographic structure of the steel, with good toughness, and is suitable for use as steel for wind turbine main shaft bearings. However, carburized steel has a high alloy content, especially a high content of precious metal Ni, and subsequent carburizing treatment is required. Although this patent uses vacuum degassing + continuous casting process to replace the electroslag remelting process, it optimizes the process to a certain extent and reduces production costs, but the cost is still high. If high-carbon bearing steel is used, the production cost can be further significantly reduced, but the use of vacuum degassing + continuous casting process to produce high-carbon bearing steel for wind turbine main shaft bearings has not yet been made public. Summary of the invention

[0007] The purpose of the present invention is to provide a high-carbon bearing steel for the rolling elements of the main shaft bearing of a wind turbine and a preparation method thereof, and to develop a production method of vacuum degassing + continuous casting process on the basis of meeting the quality requirements of steel for the rolling elements of the main shaft bearing of a wind turbine, so as to reduce the production cost of the product and make it more competitive in the market.

[0008] The technical solution of the present invention is:

[0009] The chemical composition of a high carbon bearing steel for a main shaft bearing rolling element of a wind turbine generator is C: 0.90-1.05%, Si: 0.20-0.40%, Mn: 0.60-0.80%, Cr: 1.65-1.90%, Mo: 0.20-0.35%, Ni≤0.25%, Al≤0.05%, P≤0.010%, S: 0.005-0.015%, Cu≤0.20%, Ca≤0.0010%, Ti≤0.0015%, O≤0.0008%, and the balance is Fe and unavoidable impurities. The main chemical composition design basis of the steel of the present invention is as follows:

[0010] 1) Determination of C content

[0011] In high carbon bearing steel, the carbon content is generally about 1.0%, which is one of the most important elements to ensure the hardenability, hardness and wear resistance of bearing steel. However, no matter how high the carbon content is, it has little effect on the hardness, but it is easy to produce carbides of bearing steel and reduce the toughness of bearing steel. The C content of the present invention is the same as that of the traditional high carbon chromium bearing steel GCr15, and the range is determined to be 0.90-1.05%.

[0012] 2) Determination of Si content

[0013] Adding Si to steel can strengthen ferrite, improve strength, elastic limit and hardenability, but Si increases the overheating sensitivity, cracking and decarburization tendency in the steel. The Si content of the present invention is determined to be in the range of 0.20-0.40%.

[0014] 3) Determination of Mn content

[0015] Mn, as a deoxidizing element in the steelmaking process, can improve the hardenability of steel. Mn can also fix the form of sulfur in the steel and form MnS and (Fe, Mn)S, which are less harmful to the performance of the steel, and reduce or inhibit the production of FeS. Therefore, a small amount of manganese in the steel can improve the purity and performance of the steel. However, if the Mn content in the steel is too high, a more obvious temper brittleness phenomenon will occur. In addition, Mn has the effect of promoting grain growth, which will lead to an increase in the overheating sensitivity and crack tendency of the steel, and a decrease in dimensional stability, which will have an adverse effect on customer use. The range of the Mn content of the present invention is determined to be 0.60-0.80%.

[0016] 4) Determination of Cr content

[0017] Cr is a carbide-forming element that can improve the hardenability, wear resistance and corrosion resistance of steel. However, if the Cr content is too high, it will combine with the carbon in the steel to easily form large carbides. Such insoluble carbides reduce the toughness of the steel and shorten the life of the bearing. The Cr content of the present invention is designed to be within the range of 1.65-1.90%.

[0018] 5) Determination of Al content

[0019] Al is added as a deoxidizing element in steel. In addition to reducing the dissolved oxygen in molten steel, Al and N form dispersed and fine aluminum nitride inclusions to refine the grains. However, when the Al content is too high, large particles of Al2O3 and other brittle inclusions are easily formed during the molten steel smelting process, which reduces the purity of the molten steel and affects the service life of the finished product. The range of the Al content in the present invention is determined to be ≤0.05%.

[0020] 6) Determination of Mo content

[0021] Molybdenum can refine the grains of steel, improve hardenability and heat resistance, and maintain sufficient strength and creep resistance at high temperatures. However, molybdenum is a ferrite-forming element. When the molybdenum content is high, ferrite delta phase or other brittle phases are likely to appear, which reduces toughness. The Mo content of the present invention is determined to be within the range of 0.20-0.35%.

[0022] 7) Determination of Ca content

[0023] The Ca content will increase the number and size of the point oxides in the steel. At the same time, due to the high hardness and poor plasticity of the point oxides, they do not deform when the steel is deformed, and are prone to form gaps at the interface, which deteriorates the performance of the steel. The range of the Ca content in the present invention is determined to be ≤0.001%.

[0024] 8) Determination of Ti content

[0025] Ti and N elements can form titanium nitride inclusions. Due to their high hardness and sharp corners, they are prone to cause stress concentration during bearing operation, which has a great impact on bearing life. Therefore, Ti≤0.0015%

[0026] 9) Determination of O content

[0027] The oxygen content represents the total amount of oxide inclusions. Oxide brittle inclusions limit the service life of the finished product. A large number of tests have shown that reducing the oxygen content is significantly beneficial to improving the purity of steel, especially reducing the content of brittle oxide inclusions in steel. The range of the oxygen content in the present invention is determined to be O≤0.0008%.

[0028] 10) Determination of P and S content

[0029] The P element causes element segregation during the solidification of steel. It dissolves in ferrite to make the grains distorted and coarse, and increases cold brittleness. Therefore, P is determined to be ≤ 0.010%. The S element easily makes the steel hot brittle, reduces the ductility and toughness of the steel, and the formed sulfide also destroys the continuity of the steel. However, S is beneficial to the cutting of the steel while reducing the strength of the steel. Therefore, S is determined to be: 0.005-0.015%.

[0030] The steel of the present invention further meets the following testing requirements:

[0031] Microscopic inclusions include plastic inclusions of type A and C and brittle inclusions of type B and D. Brittle inclusions are hard particles in steel, which will cause stress concentration when the bearing is running. At the same time, they are easy to separate from the matrix and produce cracks during the deformation of the steel, which will further aggravate the stress concentration and easily cause cracking. The larger the inclusion particles and the longer the length, the greater the harm. Plastic inclusions are soft particles in steel, which are not easy to separate from the matrix during the deformation of the steel, so they are less harmful.

[0032] The microscopic brittle inclusions in the steel structure of the present invention are small: B fine series ≤1.0 grade, B coarse series ≤0.5 grade, D fine series ≤1.0 grade, D coarse series ≤0.5 grade, DS series ≤1.0 grade, and the specific requirements are shown in Table 1 below. However, the macroscopic inclusions significantly reduce the wear resistance of the steel, causing serious stress concentration and easily causing early failure of the bearing during use. The macroscopic defects of the present invention require the use of SE9 1927 method for water immersion high-frequency flaw detection, requiring that the total ultrasonic defect index is not allowed to exceed 5mm / dm 3 The maximum length of a single ultrasonic defect is not allowed to exceed 2mm.

[0033] Table 1

[0034]

[0035] The uniformity and density of the macrostructure of steel have an impact on the life of the bearing. The macrostructure of steel adopts GB / T1979 to grade the macrostructure of steel, requiring central porosity ≤1.0 level, general porosity ≤1.0 level, ingot segregation ≤1.0 level, central segregation ≤1.0 level, and shrinkage cavities, cracks and subcutaneous bubbles are not allowed.

[0036] As the rolling element of the main shaft bearing of wind turbines, the surface of the steel needs to have good wear resistance and hardness after heat treatment, and the core needs to withstand a large impact load, so requirements are put forward for the mechanical properties of the steel: its end quenching J1.5 ≥ 61HRC, and the impact performance AKU requirement of the steel core at room temperature ≥ 60J.

[0037] To ensure the performance of steel, the metallographic structure required by the present invention is: the metallographic structure of the surface after hot rolling is sorbite structure, to prevent the proportion of sorbite structure from being too large and affecting the subsequent spheroidizing annealing treatment, the thickness of the sorbite structure is within 0.3%D (D is the diameter of the steel), and the core structure is pearlite structure; the metallographic structure after heat treatment is spherical carbide particles, and the spheroidization rate of carbide particles on the cross section of the round steel is 100%. In addition, in order to reduce the segregation of steel, the invention steel is required to test the carbide network, band, liquid separation and micropores according to GB / T18254-2016, among which the carbide network is ≤2.0 level, the carbide band is ≤2.0 level, and carbide liquid separation and micropores are not allowed.

[0038] A production method of high carbon bearing steel for rolling elements of wind turbine main shaft bearings:

[0039] 1. Molten steel smelting

[0040] Primary refining: The final carbon content of the steel produced during primary refining is controlled at 0.15-0.25% to prevent overoxidation of the molten steel, and the final phosphorus content is controlled at ≤0.015%;

[0041] Refining: Deoxidation is carried out during the process, slag is formed on the surface of the molten steel, deep precipitation deoxidation of the molten steel is adopted, diffusion deoxidation of the molten steel surface is adopted, bottom blowing argon is used to stir the molten steel to make inclusions float to the surface slag, the temperature of the refining furnace is controlled at 1520-1650℃, the time of the whole refining process is controlled at ≥50min, and the temperature of the molten steel is controlled at 1535℃-1575℃ at the end of refining; alloys are added in the early stage of the process to adjust the manganese and chromium content;

[0042] Vacuum degassing: After refining, high vacuum degassing treatment is carried out. After the vacuum treatment, the sulfur content in the molten steel is adjusted to the set range. At the same time, a covering agent is added to the surface of the molten steel to prevent the surface of the molten steel from being exposed to prevent oxidation of the molten steel. Argon gas is used to stir the molten steel and the molten steel is soft-blown to promote the floating of inclusions. At the end of vacuum degassing, the temperature of the molten steel is controlled at 1485℃-1525℃;

[0043] Continuous casting: The entire continuous casting process is protected to prevent oxidation of molten steel, using electromagnetic stirring, induction heating of the tundish and soft pressure reduction;

[0044] 2. Continuous Casting Billet Rolling

[0045] Continuous casting billet heating: The continuous casting billet is sent to the heating furnace hot, and the structure is completely austenitized and homogenized;

[0046] Continuous casting billet rolling: After descaling, the continuous casting billet begins rolling in the austenite single phase area, and is rolled alternately through multiple horizontal and vertical rolling mills. The deformation amount of each pass is controlled at 12%-18%. During the rolling process, the steel is water-cooled for multiple times, and the cooling rate is controlled at 20℃-30℃ / s. The final rolling temperature is controlled within the temperature range of the two-phase area where austenite and carbide precipitate. The steel is deformed in the two-phase area so that the first precipitated carbides and the unrecrystallized austenite are simultaneously subjected to plastic processing;

[0047] Cooling after rolling: After the final rolling, the steel is water-cooled, and the cooling rate is controlled at 40℃-50℃ / s, so that the surface temperature of the steel is within the range of 580℃-650℃ after the water-cooling. The steel is quickly cooled to quickly jump out of the precipitation area of ​​a large number of secondary cementite (the carbide precipitation in the final rolling stage and after rolling refers to the precipitation of secondary cementite), thereby improving the carbide network. The steel is then cooled on a cooling bed. The surface is rapidly cooled to produce martensite structure, and then the surface metallographic structure is transformed into sorbite structure due to the self-tempering situation. The thickness of the sorbite structure is ≤0.3%D, where D is the diameter of the steel, and the core is pearlite structure.

[0048] 3. Spheroidizing annealing

[0049] The steel is spheroidized annealed in a heating furnace with a protective atmosphere. The steel is heated to a temperature range of 10-20°C above Acm and kept warm, so that 70-90% of the cementite in the steel is dissolved in the austenite. The steel is then furnace-cooled to a temperature range of 20-30°C below Acm and kept warm, so that the carbides are spheroidized. Finally, the steel is cooled to 650±(0-10)°C and taken out of the furnace, so that the remaining cementite that is not completely austenitized is spheroidized. The spheroidization rate of the final finished steel is 100%.

[0050] As one of the preferred embodiments of the present application, in the primary refining step, the steel is tapped by slag blocking, and the slag removal is performed immediately after the tapping is completed; in the refining step, aluminum wire and aluminum particles are used for strong deoxidation: the aluminum wire enters the deep part of the molten steel for precipitation deoxidation, and the aluminum particles diffuse deoxidize on the surface of the molten steel. When the chemical equivalent of aluminum in the molten steel exceeds oxygen, clustered Al2O3 non-metallic inclusions that are insoluble in the molten steel and have a density less than that of the molten steel will be formed in the molten steel. Large-sized clustered Al2O3 will quickly float to the slag on the surface of the molten steel. The number of temperature measurement and sampling of the refining furnace is controlled at 3-5 times, and no alloy is allowed to be added within 20 minutes before the end of refining to prevent the newly generated inclusions from being fully absorbed by the slag and affecting the purity of the molten steel. In the vacuum degassing step, a VD furnace and / or an RH furnace is used to vacuum degas the molten steel, the vacuum degree is ≤133Pa, and the vacuum degree is maintained for ≥15min. After the vacuum treatment, a pyrite wire is fed to adjust the sulfur content, and carbonized rice husks are used as a surface covering agent for the molten steel.

[0051] As one of the preferred embodiments of the present application, in the continuous casting step, the superheat of the molten steel is reduced and the segregation of the ingot is improved. The continuous casting tundish stopper uses an argon-blown stopper, and the sealing of the stopper head must be ensured to be good. Before pouring, the sealing of the argon-blowing pipelines in the impact zone and the tundish pouring zone and the accuracy of the argon-blowing instrument must be checked, and the argon-blowing protection of the tundish before the large ladle is poured and the secondary oxidation prevention of the tundish during the pouring process must be done well. The continuous casting tundish stopper uses an argon-blown stopper, the tundish superheat △T≤18℃, the molten steel volume in the tundish is 30-35 tons, eight-roll light pressing is used, the cumulative pressing amount is 16.5mm, the 8-time distribution amount is 0.5mm-1mm-3mm-3mm-2.5mm-2.5mm-2mm-2mm, the continuous casting pouring pulling speed is 0.45-0.55min / m, and the remaining steel in the ladle is not less than 5 tons.

[0052] As one of the preferred embodiments of the present application, in the continuous casting step, large-section continuous casting is adopted, and the cross-sectional size of the continuous casting billet is greater than 400mm×400mm, ensuring that the steel compression ratio is greater than 6.

[0053] As one of the preferred embodiments of the present application, in the continuous casting billet heating step, the temperature of the preheating section is controlled at 700-850°C, the temperature of the heating section is controlled at 1100-1250°C, and the temperature of the soaking section is controlled at 1150-1250°C, so as to ensure that the billet is sufficiently and evenly heated, thereby improving the carbide segregation of the steel and eliminating the carbide liquid precipitation. At the same time, in order to prevent the generation of micropores and excessive decarburization due to excessive heating time, the total heating time is controlled at 10-15 hours.

[0054] As one of the preferred embodiments of the present application, in the continuous casting billet rolling step, the starting rolling temperature is controlled at 1000-1100°C, four water tanks are used continuously during the rolling process, water ring spray cooling is adopted, and the water flow intensity is 200m 3 / h or more, the final rolling temperature is controlled at 800℃-830℃, which is within the temperature range of the two-phase region of austenite and carbide (the temperature range of carbide precipitation is 780℃-850℃). Rolling within this temperature range allows the steel to deform through the two-phase region, so that the first precipitated carbides and the unrecrystallized austenite are simultaneously plastically processed, which refines the grains, reduces carbide focusing, and improves carbide segregation in steel. In the post-rolling cooling stage, three-stage water tanks are used continuously, and water ring spray cooling is adopted, with a water flow intensity of 300m 3 / h or more.

[0055] As one of the preferred embodiments of the present application, in the spheroidizing annealing stage, the steel is heated to 820±(0~10)℃ and kept warm for 8-10 hours, then the steel is furnace cooled to 780℃±(0~10)℃ and kept warm for 4-6 hours, and finally cooled with the furnace for 4-6 hours to 650±(0~10)℃ and taken out of the furnace.

[0056] The production process characteristics of this application are as follows:

[0057] 1. From the perspective of manufacturing technology, the use of vacuum degassing and continuous casting production technology improves production efficiency, realizes large-scale production, and is conducive to improving material composition and product quality stability.

[0058] 2. In order to improve the plasticity and toughness of steel, the composition is specially designed to better meet the use of high-carbon bearings for rolling elements of wind turbine main shaft bearings.

[0059] 3. Improve the carbide network of steel by adopting specific rolling and cooling processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 The metallographic structure diagram of the hot-rolled surface troostite structure + core pearlite structure of the steel of the present invention;

[0061] Figure 2 This is the spheroidized structure diagram of the steel material of the present invention. DETAILED DESCRIPTION

[0062] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0063] The chemical composition (wt %) of GCr15 produced by the various embodiments of the present invention and (for comparison) the electroslag remelting process currently used on the market is shown in Table 2-1 and Table 2-2.

[0064] Table 2-1

[0065]

[0066] Table 2-2

[0067]

[0068] Tables 3 to 5 are comparisons of the inspection results of each embodiment and the above-mentioned comparative steel in terms of non-metallic inclusions, carbides, microscopic pores, and low magnification.

[0069] Table 3 Non-metallic inclusion detection of various examples and comparative steels

[0070]

[0071] Table 4 Carbide bands, carbide networks, carbide liquid separation and micropores of various examples

[0072] Carbide Network Carbide ribbon Carbide liquid precipitation Micropores Embodiment 1 of the present invention 1.5 1.0 0 none Embodiment 2 of the present invention 1.5 1.5 0 none Embodiment 3 of the present invention 1.5 1.5 0 none Contrast steel 1.5 1.0 0 none

[0073] Table 5 Macro data of steel materials in various examples

[0074] Loose center Generally loose Ingot segregation Center Segregation crack Shrinkage Subcutaneous bubbles Embodiment 1 of the present invention 0.5 0.5 0.5 0.5 none none none Embodiment 2 of the present invention 0.5 0.5 0.5 0.5 none none none Embodiment 3 of the present invention 0.5 0.5 0.5 0.5 none none none Contrast steel 0.5 0.5 0.5 0.5 none none none

[0075] Table 6, end quenching and impact work of steel in various examples

[0076] J1.5,HRC Heart normal temperature impact energy AKU, J Embodiment 1 of the present invention 63 82 Embodiment 2 of the present invention 62.5 88 Embodiment 3 of the present invention 62.5 95 Contrast steel 61 58

[0077] The present invention is further described in detail below with reference to the embodiments.

[0078] The manufacturing process of high carbon bearing steel for rolling elements of main shaft bearings of wind turbines in the embodiment is to produce steel by adopting top and bottom combined blowing converter BOF (high power electric arc furnace EAF) - ladle refining furnace LF - vacuum circulating degassing furnace RH (VD furnace) - large section continuous casting CCM - hot delivery of continuous casting billet - hot rolling into product - finishing - spheroidizing annealing process.

[0079] Specifically, high-quality molten iron, scrap steel and raw and auxiliary materials are selected during smelting, and high-quality deoxidizers and refractory materials are selected. In the production process of the electric furnace / converter, the high-quality molten iron and high-quality alloy are proportioned according to the element composition of the present invention, and the raw materials are loaded into the electric furnace or converter, and oxygen is blown to assist melting. The steel tapping end point C of the three embodiments is respectively controlled at 0.15-025%, the end point P is controlled at ≤0.015%, the steel tapping temperature is 1620℃-1650℃, Al iron is added during the steel tapping process for pre-deoxidation, and slag removal is performed after steel tapping, and then re-slag is made in the refining furnace. Aluminum wire and aluminum particles are used for diffusion and precipitation deoxidation during the refining process. The entire refining time is controlled between 60-80min. The continuous casting superheat is controlled within ≤18℃, and the continuous casting drawing speed is controlled at 0.45-0.55m / min. The continuous casting billet is heated in the walking beam furnace for about 13 hours. The actual temperature of the soaking section is controlled within the range of 1220±10℃. The final rolling temperature is controlled by water cooling during the rolling process. The final rolling temperature is controlled at 800-830℃. After rolling, water cooling is continued to be used to control the red-return temperature of the steel. The red-return temperature is controlled within the range of 590±20℃. The metallographic structure after rolling is sorbite on the surface and pearlite in the core. See Figure 1 The subsequent spheroidizing annealing process of the steel strictly complies with the aforementioned spheroidizing annealing process requirements of the steel to ensure that the steel in the embodiment is 100% spheroidized. The specific spheroidized structure is shown in Figure 2 .

[0080] Combined with the inspection results of Table 2-1, Table 2-2, Table 3, Table 4 and Table 5:

[0081] From the perspective of composition, the main chemical composition difference between the present invention and the comparative steel is that there is a significant difference in the composition of Mn, Cr and Mo, the elements that affect the hardenability and toughness of steel. The present invention reasonably designs the chemical composition, and its surface hardenability and core impact work are better, thereby improving the toughness and hardenability of the material, so that it can better meet the requirements of high-carbon bearing steel for the rolling element of the main shaft bearing of wind turbines. From the results of low-power, microscopic pores, and carbide liquid analysis, the indicators of the present invention and the comparative steel are equivalent. From the results of non-metallic inclusions and carbide bands and meshes, the present invention is slightly worse than the GCr15 comparative steel produced by electroslag remelting. Although the electroslag remelting process can significantly improve the purity of the material and improve the segregation of the steel, its process is complicated, the production efficiency is low, and the cost is high. The present invention adopts vacuum degassing and continuous casting process for production, which has a significant advantage in production efficiency and cost. Although the corresponding indicators are slightly worse than those of the products produced by the electroslag remelting process, it can also fully meet the requirements of high-carbon bearing steel for the rolling element of the main shaft bearing of wind turbines, and has a very large competitive advantage.

[0082] Based on the above analysis, the high carbon bearing steel for the rolling element of the main shaft bearing of the wind turbine in each embodiment of the present invention has the following differences compared with the current products:

[0083] 1. The main chemical composition design is different.

[0084] 2. During the production process, the purity of molten steel is controlled, and long-term high-temperature diffusion is adopted, while controlled rolling and controlled cooling processes are coordinated to ensure the purity and segregation index of the steel.

[0085] 3. The production process is different. The vacuum degassing + continuous casting process is used to replace the current electroslag remelting process. On the premise of fully meeting the requirements of steel, it greatly increases production sales and reduces production costs, and has strong market competitiveness.

[0086] In summary, the present invention relates to a high-carbon bearing steel for rolling elements of a wind turbine main shaft bearing and a production method thereof. Through a new design of the chemical composition of the steel, a high-efficiency, high-capacity, and low-cost process route of vacuum degassing, continuous casting, and rolling is adopted, and key processes are optimized, studied, and controlled, so that the steel has a high purity and a good segregation control quality level, making it more competitive in production efficiency, production cost, and product quality stability.

[0087] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

[0088] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A high carbon bearing steel for a rolling element of a main shaft bearing of a wind turbine generator, characterized in that: The mass percentage of its element composition is: C: 0.90-1.05%, Si: 0.20-0.40%, Mn: 0.60-0.80%, Cr: 1.65-1.90%, Mo: 0.20-0.35%, Ni≤0.25%, Al≤0.05%, P≤0.010%, S: 0.005-0.015%, Cu≤0.20%, Ca≤0.0010%, Ti≤0.0015%, O≤0.0008%, the balance is Fe and unavoidable impurities; The metallographic structure of the steel surface after hot rolling is sorbite structure, and the core structure is pearlite structure; the metallographic structure after spheroidizing annealing treatment is spheroidal carbide particles, and the spheroidization rate of carbide particles on the cross section of round steel is 100%; The steel production method comprises:

1. Molten steel smelting Primary refining: The final carbon content of the steel produced during primary refining is controlled at 0.15-0.25% to prevent overoxidation of the molten steel, and the final phosphorus content is controlled at ≤0.015%; Refining: Deoxidation is carried out during the process, slag is formed on the surface of the molten steel, deep precipitation deoxidation of the molten steel is adopted, diffusion deoxidation of the molten steel surface is adopted, bottom blowing argon is used to stir the molten steel to make inclusions float to the surface slag, the temperature of the refining furnace is controlled at 1520-1650℃, the time of the whole refining process is controlled at ≥50min, and the temperature of the molten steel is controlled at 1535℃-1575℃ at the end of refining; alloys are added in the early stage of the process to adjust the manganese and chromium content; Vacuum degassing: After refining, high vacuum degassing treatment is carried out. After the vacuum treatment, the sulfur content in the molten steel is adjusted to the set range. At the same time, a covering agent is added to the surface of the molten steel to prevent the surface of the molten steel from being exposed. Argon gas is used to stir the molten steel to promote the floating of inclusions. At the end of vacuum degassing, the temperature of the molten steel is controlled at 1485℃-1525℃; Continuous casting: The entire continuous casting process is protected to prevent oxidation of molten steel, using electromagnetic stirring, induction heating of the tundish and soft pressure reduction; 2. Continuous Casting Billet Rolling Continuous casting billet heating: The continuous casting billet is sent to the heating furnace hot, and the structure is completely austenitized and homogenized; Continuous casting billet rolling: the rolling temperature is controlled at 1000-1100℃, four water tanks are used continuously during the rolling process, water ring spray cooling is adopted, and the water flow intensity is 200m 3 / h or more, the final rolling temperature is controlled at 800℃-830℃; in the cooling stage after rolling, three-stage water tanks are used continuously, water ring spray cooling is adopted, and the water flow intensity is 300m 3 / h or more; after the continuous casting billet is descaled, it starts rolling in the austenite single phase area, and is rolled alternately through multiple horizontal and vertical rolling mills, with the deformation amount of each pass controlled at 12%-18%. During the rolling process, the steel is water-cooled for multiple times, and the cooling rate is controlled at 20℃-30℃ / s. The final rolling temperature is controlled within the temperature range of the two-phase area where austenite and carbide precipitate. The steel is deformed in the two-phase area so that the first precipitated carbides and the unrecrystallized austenite are simultaneously subjected to plastic processing; Cooling after rolling: After the final rolling, the steel is water-cooled, and the cooling rate is controlled at 40℃-50℃ / s, so that the surface temperature of the steel is in the range of 580℃-650℃ after the water-cooling, so that the steel can quickly jump out of the precipitation area of ​​a large number of secondary cementite, and then the steel is cooled on the cooling bed. The rapid cooling after rolling produces martensite structure on the surface, and then the surface metallographic structure is transformed into sorbite structure due to self-tempering. The thickness of sorbite structure is ≤0.3%D, D is the diameter of the steel, and the core is pearlite structure; 3. Spheroidizing annealing The steel is spheroidized annealed in a heating furnace with a protective atmosphere. The steel is heated to 820±(0~10)℃ and kept warm for 8-10 hours to cause 70-90% of the cementite in the steel to dissolve in the austenite. The steel is then furnace cooled to 780±(0~10)℃ and kept warm for 4-6 hours to spheroidize the carbides. Finally, the steel is cooled in the furnace for 4-6 hours to 650±(0~10)℃ before being taken out of the furnace to cause the remaining cementite that has not been completely austenitized to spheroidize.

2. The high carbon bearing steel for rolling elements of the main shaft bearing of a wind turbine generator according to claim 1 is characterized in that: The thickness of the sorbite structure on the surface of the steel after hot rolling is ≤0.3%D, where D is the diameter of the steel, and the rest is pearlite structure.

3. The high carbon bearing steel for rolling elements of the main shaft bearing of a wind turbine generator according to claim 1, characterized in that: The round steel end quenching J1.5 ≥ 61HRC, the impact performance AKU requirement of the steel core at room temperature is ≥ 60J.

4. The high carbon bearing steel for rolling elements of the main shaft bearing of a wind turbine generator according to claim 1, characterized in that: Micro inclusions are tested according to GB / T 10561 A method, B fine series ≤1.0, B coarse series ≤0.5, D fine series ≤1.0, D coarse series ≤0.5, DS series ≤1.0; Macro defects are inspected by water immersion high frequency flaw detection using the SE9 1927 method, and the total ultrasonic defect index does not exceed 5mm / dm 3 , the maximum length of a single ultrasonic defect does not exceed 2mm; Macrostructure requirements GB / T 1979 is used to grade steel macrostructures, with central porosity ≤1.0, general porosity ≤1.0, ingot segregation ≤1.0, central segregation ≤1.0, and no shrinkage cavities, cracks or subcutaneous bubbles. According to GB / T 18254-2016, the carbide network, banding, liquid separation and micropores are inspected. The carbide network is ≤ grade 2.0, the carbide banding is ≤ grade 2.0, and there is no carbide liquid separation or micropores.

5. The high carbon bearing steel for rolling elements of the main shaft bearing of a wind turbine according to claim 1, characterized in that: In the primary refining step, the steel is tapped by slag blocking, and the slag removal is carried out immediately after the tapping is completed; in the refining step, aluminum wire and aluminum particles are used for strong deoxidation: the aluminum wire enters the deep part of the molten steel for precipitation deoxidation, and the aluminum particles diffuse deoxidize on the surface of the molten steel, so that the chemical equivalent of aluminum in the molten steel exceeds that of oxygen; the number of temperature measurement and sampling in the refining furnace is controlled at 3-5 times, and no alloy is allowed to be added within 20 minutes before the end of refining; in the vacuum degassing step, a VD furnace and / or an RH furnace is used to vacuum degas the molten steel, the vacuum degree is ≤133Pa, and the vacuum degree is maintained for ≥15min. After the vacuum treatment is completed, a pyrite wire is fed to adjust the sulfur content, and carbonized rice husks are used as a surface covering agent for the molten steel.

6. The high carbon bearing steel for rolling elements of the main shaft bearing of a wind turbine according to claim 1, characterized in that: In the continuous casting step, an argon-blown stopper rod is used for the continuous casting tundish plug rod, the tundish superheat △T≤18°C, the amount of molten steel in the tundish is 30-35 tons, eight-roller light pressing is adopted, the cumulative pressing amount is 16.5mm, the 8-time distribution amount is 0.5mm-1mm-3mm-3mm-2.5mm-2.5mm-2mm-2mm, the continuous casting pouring speed is 0.45-0.55min / m, and the remaining steel amount in the ladle is not less than 5 tons.

7. The high carbon bearing steel for rolling elements of the main shaft bearing of a wind turbine according to claim 1, characterized in that: In the continuous casting step, large-section continuous casting is adopted, and the cross-sectional size of the continuous casting billet is greater than 400mm×400mm, ensuring that the compression ratio of the steel is greater than 6.

8. The high carbon bearing steel for rolling elements of a main shaft bearing of a wind turbine according to claim 1, characterized in that: In the continuous casting billet heating step, the preheating section temperature is controlled at 700-850°C, the heating section temperature is controlled at 1100-1250°C, the soaking section temperature is controlled at 1150-1250°C, and the total heating time is controlled at 10-15 hours.