MIM-based iron-based alloy powder and composite second-phase reinforced stainless steel injection molding preparation method
By using specific iron-based alloy powders and process steps in MIM technology to form multiple nanosecond phases, the problem of insufficient yield strength of stainless steel in MIM technology is solved, and high strength and high elongation stainless steel materials are achieved, suitable for lightweighting equipment.
Patent Information
- Application Number
- CN202410971605.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing MIM technology is difficult to break through the yield strength of stainless steel 2000MPa limit, limiting its development in some areas in lightweight and high-strength toughness applications, especially in folding screen mobile phones and other devices.
Using MIM-based iron-based alloy powder, a variety of nanosecond phases are formed through specific component ratios and process steps such as powder pretreatment, feeding preparation, injection molding, degreasing, sintering, solid solution, deep cooling and aging treatment. Refine the grains and improve the strength of the material.
The yield strength is close to or exceeding 2000MPa, with an elongation of ≥5%, meeting higher strength and toughness and lightweight requirements, and is suitable for folding screen mobile phones and other devices.
Smart Images

Figure CN118910516A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the fields of materials and MIM, and in particular to a method for preparing iron-based alloy powder and composite second-phase reinforced stainless steel by injection molding based on MIM. Background Art
[0002] Maraging steel uses nickel as the primary alloying element to form an Fe-Ni martensite matrix with excellent strength and toughness. During aging at 450-550°C, alloying elements such as Co, Mo, and Ti precipitate intermetallic compounds (such as Ni3Ti and Ni3Mo) from the supersaturated Fe-Ni martensite matrix. Simultaneously, stable reverse-transformed austenite forms between the martensite laths, achieving an excellent balance of strength and toughness. This steel has been extensively developed and used in both military and commercial applications.
[0003] Powder injection molding (MIM) technology uses metal powder as raw material, and produces metal materials and composite materials through mixing, injection, degreasing, and sintering. Compared with traditional processes such as forging and die-casting, it has the advantages of low cost, applicability to various materials, and the ability to produce products of various complex shapes. It is used in consumer electronics, automobiles, and medical fields. At the same time, there are few reports on the development of ultra-high-strength steel using MIM technology. Due to the enlarged grain size during the sintering process and the difficulty in controlling the precipitation of the second phase, it is difficult to break through the yield strength of 2000Mpa. This limits its application in many fields and also hinders the lightweighting and thinning process of foldable screen mobile phones. It is necessary to find a new type of stainless steel material with higher strength to meet the growing demand. Summary of the Invention
[0004] The first object of the present invention is to provide an MIM-based iron-based alloy powder, which, when combined with the MIM process, can produce stainless steel products with high yield strength and large elongation, thereby meeting the requirements of higher strength, toughness and lightweight.
[0005] The technical solution for achieving the first object of the present invention is: the iron-based alloy powder based on MIM in the present invention includes the following components in weight percentage: C: 0.05-0.5%; Cr: 2.0-6.0%; Ni: 8.0-12.0%; Co: 13.0-17.0%; Mo: 4.0-7.0%; V: 0.05-0.20%; Nb: 0.1-1%, and the balance is Fe; the total content of O, N, P, and S does not exceed 0.36%.
[0006] As an optimized design, the iron-based alloy powder based on MIM in the present invention includes the following components in weight percentage: C: 0.05-0.3%; Cr: 3.0-5.0%; Ni: 9.0-11.0%; Co: 13.0-15.0%; Mo: 4.0-6.0%; V: 0.3-0.5%; Nb: 0.2-0.8%, and the balance is Fe, O≤0.35%, N≤0.005%, P≤0.01%, and S≤0.005%.
[0007] The second object of the present invention is to provide a method for preparing composite second-phase reinforced stainless steel by injection molding, which can form multiple second phases in the above-mentioned iron-based alloy powder during the MIM process, thereby achieving the purpose of strengthening the stainless steel.
[0008] The technical solution for achieving the second object of the present invention is: the preparation method of composite second phase strengthened stainless steel injection molding in the present invention comprises the following steps:
[0009] S1. Powder surface pretreatment: The iron-based alloy powder according to claim 1 or 2 is fully mixed with a surface modifier and then dried to form a pre-prepared powder; wherein the surface modifier is polyethylene glycol dipropylene oxide, and the surface modifier is added according to 1 to 5‰ of the weight of the iron-based alloy powder;
[0010] S2. Feed material preparation: uniformly mix the pre-prepared powder and binder to prepare feed material for metal injection molding;
[0011] S3, injection molding: the feed is injected into the mold to obtain a green body;
[0012] S4, catalytically degreasing the green body to obtain a degreased body;
[0013] S5, thermally debinding the degreased blank and vacuum sintering the degreased blank to obtain a sintered blank;
[0014] S6. The sintered blank is subjected to solution treatment, cryogenic treatment and aging treatment in sequence to obtain composite second-phase strengthened stainless steel.
[0015] Furthermore, the above-mentioned solution treatment is carried out at 1050-1150°C for 1 hour to 5 hours; the deep cold treatment is carried out at ≤-196°C for 1 hour to 10 hours; and the aging treatment is carried out at 500-560°C for 1 hour to 10 hours.
[0016] Furthermore, the particle size of the iron-based alloy powder in the above step S1 is controlled to be D50: 2 to 8 μm.
[0017] Furthermore, in the above step S2, the pre-prepared powder and the binder are mixed in a volume ratio of 1:1 to 3:1, and the feed is prepared using a banburying granulator. The banburying temperature is 190 to 200°C, the banburying time is 1.5 to 2 hours, and the feed particle size is Φ2.0 to 4.0 mm.
[0018] Furthermore, during the injection molding in the above step S3, the barrel temperature is 175-185°C, the nozzle temperature is 190-200°C, and the mold temperature is 90-120°C.
[0019] Furthermore, in the above step S4, nitric acid is used for catalytic degreasing, and the degreasing process is as follows: temperature 100-120° C., time 6 hours, and atmosphere is nitrogen with a purity of 99.999%.
[0020] Furthermore, in the above step S5, the vacuum sintering is carried out at a temperature of 1200-1380°C for 1-10 hours, with a vacuum degree of 10 -2 Pa.
[0021] The present invention has positive effects: (1) The present invention generates a variety of strong carbides and precipitates nano-second phases by adding Cr, Nb, and C elements through solid solution deep cold aging treatment, which greatly improves the strength and toughness of the material.
[0022] (2) The present invention hinders the further increase of grains during sintering densification and solution treatment by adding appropriate amounts of Nb and V elements, effectively refining the grains and increasing the strength and toughness of the material.
[0023] (3) The yield strength of various second-phase reinforced high-strength iron-based alloys prepared by the present invention can approach or exceed 2000 MPa, and the elongation is ≥5%, which meets the requirements of folding screen mobile phone hinges for higher toughness and lightweight materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments and in conjunction with the accompanying drawings, wherein
[0025] Figure 1 This is a metallographic photograph of the composite second phase strengthened stainless steel prepared in Example 1 of the present invention;
[0026] Figure 2 This is a metallographic photograph of the composite second phase strengthened stainless steel prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0027] (Example 1)
[0028] The iron-based alloy powder based on MIM in the present invention includes the following components in weight percentage: C: 0.05%; Cr: 3%; Ni: 9%; Co: 13%; Mo: 4%; V: 0.3%; Nb: 0.2%, and the balance is Fe; the total content of O, N, P, and S does not exceed 0.36%.
[0029] The composite second phase reinforced stainless steel injection molding preparation method of the present invention comprises the following steps:
[0030] S1. Powder surface pretreatment: The MIM-based iron-based alloy powder and the surface modifier are fully mixed in a certain proportion and then dried to form a pre-prepared powder; wherein the MIM-based iron-based alloy powder is a water-vapor atomized pre-alloyed powder with a particle size D50 of 8 μm; the surface modifier is polyethylene glycol dipropylene oxide (PEG-EP), and the amount of polyethylene glycol dipropylene oxide (PEG-EP) added is 0.3% by weight of the MIM iron-based alloy powder;
[0031] S2. Feed material preparation: The pre-prepared powder and the binder are uniformly mixed to prepare feed material for metal injection molding; wherein the pre-prepared powder and the binder are mixed in a volume ratio of 1:1, heated to 200° C. in a mixer-granulator, and mixed for 1.5 hours before extrusion, pelletizing, and granulation to obtain 3.2 mm Φ granular feed material;
[0032] S3. Injection molding: The feed material is injected into a green body; during injection molding, the barrel temperature is 175-185°C, the nozzle temperature is 195°C, and the mold temperature is 110°C;
[0033] S4, catalytically debinding the green body in a nitric acid catalytic debinding furnace at a temperature of 120° C. for 6 hours using 99.999% nitrogen gas to obtain a debinded body;
[0034] S5. Place the degreased blank into a vacuum sintering furnace for sintering at a temperature of 1380°C for 4 hours and a vacuum degree of 10 - 2 Pa, to obtain a sintered compact;
[0035] S6. The sintered blank sample is subjected to subsequent heat treatment, with a solution temperature of 1020°C and a holding time of 2 hours. The gas pressure is rapidly cooled to room temperature, and the cooling gas is nitrogen with a purity of 99.999%. The sample after solution is then cryogenically treated, with a cryogenic temperature of -196°C and a holding time of 4 hours, and then slowly heated to room temperature. Finally, the sample after cryogenic treatment is aged at an aging temperature of 500°C and a holding time of 4 hours, and then air-cooled to room temperature to obtain composite second-phase strengthened stainless steel.
[0036] (Example 2)
[0037] The iron-based alloy powder based on MIM in the present invention includes the following components in weight percentage: C: 0.05%; Cr: 3%; Ni: 9%; Co: 13%; Mo: 4%; V: 0.3%; Nb: 0.2%, and the balance is Fe; the total content of O, N, P, and S does not exceed 0.36%.
[0038] The composite second phase reinforced stainless steel injection molding preparation method of the present invention comprises the following steps:
[0039] S1. Powder surface pretreatment: The MIM-based iron-based alloy powder and the surface modifier are fully mixed in a certain proportion and then dried to form a pre-prepared powder; wherein the MIM-based iron-based alloy powder is a water-vapor atomized pre-alloyed powder with a particle size D50 of 2 μm; the surface modifier is polyethylene glycol dipropylene oxide (PEG-EP), and the amount of polyethylene glycol dipropylene oxide (PEG-EP) added is 0.3% by weight of the MIM iron-based alloy powder;
[0040] S2. Feed material preparation: The pre-prepared powder and the binder are uniformly mixed to prepare feed material for metal injection molding; wherein the pre-prepared powder and the binder are mixed in a volume ratio of 1:1, heated to 200° C. in a mixer-granulator, and mixed for 1.5 hours before extrusion, pelletizing, and granulation to obtain 3.2 mm Φ granular feed material;
[0041] S3. Injection molding: The feed material is injected into a green body; during injection molding, the barrel temperature is 175-185°C, the nozzle temperature is 195°C, and the mold temperature is 110°C;
[0042] S4, catalytically debinding the green body in a nitric acid catalytic debinding furnace at a temperature of 120° C. for 6 hours using 99.999% nitrogen gas to obtain a debinded body;
[0043] S5, put the degreased blank into the vacuum sintering furnace for sintering, the sintering temperature is 1200℃, keep warm for 4h, and the vacuum degree is 10 - 2 Pa, to obtain a sintered compact;
[0044] S6. The sintered blank sample is subjected to subsequent heat treatment, with a solution temperature of 1020°C and a holding time of 2 hours. The gas pressure is rapidly cooled to room temperature, and the cooling gas is nitrogen with a purity of 99.999%. The sample after solution is then cryogenically treated, with a cryogenic temperature of -196°C and a holding time of 4 hours, and then slowly heated to room temperature. Finally, the sample after cryogenic treatment is aged at an aging temperature of 500°C and a holding time of 4 hours, and then air-cooled to room temperature to obtain composite second-phase strengthened stainless steel.
[0045] (Example 3)
[0046] The iron-based alloy powder based on MIM in the present invention includes the following components in weight percentage: C: 0.3%; Cr: 5%; Ni: 11%; Co: 15%; Mo: 6%; V: 0.5%; Nb: 0.8%, and the balance is Fe; the total content of O, N, P, and S does not exceed 0.36%.
[0047] The composite second phase reinforced stainless steel injection molding preparation method of the present invention comprises the following steps:
[0048] S1. Powder surface pretreatment: The MIM-based iron-based alloy powder and the surface modifier are fully mixed in a certain proportion and then dried to form a pre-prepared powder; wherein the MIM-based iron-based alloy powder is a water-vapor atomized pre-alloyed powder with a particle size D50 of 2 μm; the surface modifier is polyethylene glycol dipropylene oxide (PEG-EP), and the amount of polyethylene glycol dipropylene oxide (PEG-EP) added is 0.3% by weight of the MIM iron-based alloy powder;
[0049] S2. Feed material preparation: The pre-prepared powder and the binder are uniformly mixed to prepare feed material for metal injection molding; wherein the pre-prepared powder and the binder are mixed in a volume ratio of 1:1, heated to 200° C. in a mixer-granulator, and mixed for 1.5 hours before extrusion, pelletizing, and granulation to obtain 3.2 mm Φ granular feed material;
[0050] S3. Injection molding: The feed material is injected into a green body; during injection molding, the barrel temperature is 175-185°C, the nozzle temperature is 195°C, and the mold temperature is 110°C;
[0051] S4, catalytically debinding the green body in a nitric acid catalytic debinding furnace at a temperature of 120° C. for 6 hours using 99.999% nitrogen gas to obtain a debinded body;
[0052] S5, put the degreased blank into the vacuum sintering furnace for sintering, the sintering temperature is 1200℃, keep warm for 4h, and the vacuum degree is 10 - 2 Pa, to obtain a sintered compact;
[0053] S6. The sintered blank sample is subjected to subsequent heat treatment, with a solution temperature of 1020°C and a holding time of 2 hours. The gas pressure is rapidly cooled to room temperature, and the cooling gas is nitrogen with a purity of 99.999%. The sample after solution is then cryogenically treated, with a cryogenic temperature of -196°C and a holding time of 4 hours, and then slowly heated to room temperature. Finally, the sample after cryogenic treatment is aged at an aging temperature of 500°C and a holding time of 4 hours, and then air-cooled to room temperature to obtain composite second-phase strengthened stainless steel.
[0054] The test results of the composite second phase strengthened stainless steel prepared in Examples 1 to 3 are as follows:
[0055] Density (g / cm3) Yield strength (R0.2 Mpa) Elongation (%) Example 1 7.6 1850 7 Example 2 7.65 2040 7 Example 3 7.78 2100 4
[0056] The results of the examples show that the yield strength of a variety of second-phase strengthened high-strength iron-based alloys prepared by the metal injection molding process and subsequent heat treatment process provided by the present invention can approach 2000 MPa, and Examples 2 and 3 can exceed 2000 MPa, with an elongation of ≥5%, meeting the requirements of higher strength, toughness and lightweight materials for folding screen mobile phone hinges, etc.
[0057] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An iron-based alloy powder based on MIM, characterized in that: The following components are included by weight percentage: C: 0.05~0.5%; Cr: 2.0-6.0%; Ni: 8.0-12.0%; Co: 13.0-17.0%; Mo: 4.0-7.0%; V: 0.05-0.20%; Nb: 0.1-1%, the balance is Fe; the total content of O, N, P and S does not exceed 0.36%.
2. The MIM-based iron-based alloy powder according to claim 1, characterized in that: The invention comprises the following components in weight percentage: C: 0.05-0.3%; Cr: 3.0-5.0%; Ni: 9.0-11.0%; Co: 13.0-15.0%; Mo: 4.0-6.0%; V: 0.3-0.5%; Nb: 0.2-0.8%, and the balance is Fe, O≤0.35%, N≤0.005%, P≤0.01%, and S≤0.005%.
3. A method for preparing composite second phase reinforced stainless steel by injection molding, characterized in that The following steps are involved: S1. Powder surface pretreatment: the iron-based alloy powder according to claim 1 or 2 is fully mixed with a surface modifier and then dried to form a pre-prepared powder; wherein the surface modifier is polyethylene glycol dipropylene oxide, and the surface modifier is added according to 1-5‰ of the weight of the iron-based alloy powder; S2, feed material preparation: uniformly mixing the pre-prepared powder and the binder to prepare feed material for metal injection molding; S3, injection molding: the feed is injected into the mold to obtain a green body; S4, catalytically degreasing the green body to obtain a degreased body; S5, thermally debinding the degreased blank and vacuum sintering the degreased blank to obtain a sintered blank; S6. The sintered blank is subjected to solution treatment, cryogenic treatment and aging treatment in sequence to obtain composite second phase strengthened stainless steel.
4. The method for preparing composite second phase strengthened stainless steel by injection molding according to claim 3, characterized in that: The solution treatment is carried out by keeping the temperature at 1050-1150° C. for 1 h to 5 h; the cryogenic treatment is carried out by keeping the temperature at ≤-196° C. for 1 h to 10 h; and the aging treatment is carried out by keeping the temperature at 500-560° C. for 1 h to 10 h.
5. The method for preparing composite second phase strengthened stainless steel by injection molding according to claim 3, characterized in that: The particle size of the iron-based alloy powder in step S1 is controlled within the range of D50: 2-8 μm.
6. The method for preparing composite second phase strengthened stainless steel by injection molding according to claim 3, characterized in that: In the step S2, the pre-prepared powder and the binder are mixed in a volume ratio of 1:1 to 3:1, and the feed is prepared by a banburying granulator. The banburying temperature is 190 to 200° C., the banburying time is 1.5 to 2 hours, and the feed particle size is Φ2.0 to 4.0 mm.
7. The method for preparing composite second phase strengthened stainless steel by injection molding according to claim 3, characterized in that: During the injection molding in step S3, the barrel temperature is 175-185°C, the nozzle temperature is 190-200°C, and the mold temperature is 90-120°C.
8. The method for preparing composite second phase strengthened stainless steel by injection molding according to claim 3, characterized in that: In step S4, nitric acid is used for catalytic degreasing, and the degreasing process is as follows: temperature 100-120° C., time 6 hours, and atmosphere is nitrogen with a purity of 99.999%.
9. The method for preparing composite second phase strengthened stainless steel by injection molding according to claim 3, characterized in that: In step S5, the vacuum sintering is carried out at 1200-1380°C for 1-10 hours with a vacuum degree of 10 -2 Pa.
Citation Information
Cited By
Method for repairing guide groove of piston rod of aircraft refueling exploring tube
CN119956351A
Stainless steel material for metal injection molding processing and preparation method and application thereof
CN120290988A
High-toughness ultrahigh-strength martensitic stainless steel material as well as preparation method and application thereof
CN120555917A
Low-cost ultrahigh-strength martensitic steel material as well as preparation method and application thereof
CN122013070A