Powder coating for new energy automobile electric drive system and preparation method of powder coating

By combining modified boron nitride and composite epoxy resin, the problem of poor compatibility between boron nitride and epoxy resin is solved, and the moisture and heat resistance, impact resistance and thermal stability of powder coatings in electric drive systems of new energy vehicles is improved. Enhanced insulation anti-aging properties.

CN119039856AActive Publication Date: 2024-11-29JIANGSU HUAGUANG POWDER +3

Patent Information

Application Number
CN202411294886.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-29
Estimated Expiration
2044-09-14

AI Technical Summary

Technical Problem

In the existing electric drive systems of new energy vehicles, poor compatibility between boron nitride and epoxy resin leads to internal defects of the paint, affecting the mechanical properties and overall quality.

Method used

Modified boron nitride and composite epoxy resin are used to prepare modified boron nitride by reacting aluminate coupling agent with hydroxylated boron nitride, and it is uniformly dispersed in the alumina sol, combining heptafluorodecyl Trimethoxysilane improves compatibility while introducing 4-aminophenylborate to improve thermal stability and mechanical properties.

Benefits of technology

It significantly improves the moisture and heat resistance, impact resistance and thermal stability of powder coatings, enhances the insulation and aging resistance, and improves the compatibility of boron nitride and alumina sol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005045636540000101
    Figure BDA0005045636540000101
  • Figure BDA0005045636540000111
    Figure BDA0005045636540000111
Patent Text Reader

Abstract

The invention discloses a powder coating for an electric drive system of a new energy automobile and a preparation method of the powder coating, and relates to the technical field of powder coatings. The powder coating for the electric drive system of the new energy automobile, prepared by the invention, comprises the following raw material components in parts by weight: 50-80 parts of composite epoxy resin, 10-20 parts of composite filler, 2-4 parts of a curing agent, 0.2-0.8 part of an imidazole accelerant, 1-2 parts of a flatting agent, 0.8 part of wax powder, 0.3-0.9 part of benzoin and 1-5 parts of pigment, the composite epoxy resin is obtained by carrying out mixing reaction on 2-amino-4-hydroxy-6-methylpyrimidine, a hexamethylene diisocyanate tripolymer, 4-aminophenylboronic acid pinacol ester and epoxy resin; the composite filler is obtained by mixing and reacting aluminum isopropoxide, ethyl acetoacetate, ethanol, modified boron nitride and a silane coupling agent; the modified boron nitride is aluminic acid ester coupling agent modified boron nitride.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of powder coatings, and in particular to a powder coating for an electric drive system of a new energy vehicle and a preparation method thereof. Background Art

[0002] With the rapid development of the new energy vehicle industry, higher requirements are placed on the reliability and durability of the electric drive system. The insulation materials in the electric drive system must not only provide good electrical insulation performance, but also have excellent anti-aging performance to ensure the long-term stable operation of the entire system. Powder coatings, as a commonly used insulating material, have been widely used in new energy vehicle electric drive systems due to their environmental protection and high efficiency.

[0003] At present, there are some insulating anti-aging powder coatings for new energy vehicle electric drive systems on the market. In order to improve the anti-aging properties of these coatings, researchers usually add boron nitride (BN) as a filler in the epoxy resin matrix. Boron nitride has good thermal stability, high thermal conductivity and excellent electrical insulation properties, which can significantly improve the anti-aging properties of coatings. However, the poor compatibility between boron nitride and epoxy resin is a problem that needs to be solved urgently. Boron nitride particles tend to agglomerate in the epoxy resin matrix, resulting in defects inside the coating, which affects the mechanical properties and overall quality of the final product.

[0004] Therefore, the applicant prepared a powder coating for the electric drive system of new energy vehicles to solve the above problems. Summary of the invention

[0005] In order to solve the existing technical problems, the present invention provides a powder coating for an electric drive system of a new energy vehicle. The raw material components include, by weight: 50 to 80 parts of a composite epoxy resin, 10 to 20 parts of a composite filler, 2 to 4 parts of a curing agent, 0.2 to 0.8 parts of an imidazole accelerator, 1 to 2 parts of a leveling agent, 0.8 parts of wax powder, 0.3 to 0.9 parts of benzoin, and 1 to 5 parts of a pigment;

[0006] The leveling agent is polyether-modified polydimethylsiloxane;

[0007] The curing agent is latent dicyandiamide;

[0008] The catalyst adopts an imidazole promoter.

[0009] Furthermore, the composite epoxy resin is obtained by a mixed reaction of 2-amino-4-hydroxy-6-methylpyrimidine, hexamethylene diisocyanate trimer, 4-aminophenylboronic acid pinacol ester, and epoxy resin; the epoxy resin adopts E51 type epoxy resin, whose average epoxy value is 0.51 and average hydroxyl value is 0.046; by introducing 4-aminophenylboronic acid pinacol ester into the epoxy resin, not only the thermal stability of the epoxy resin can be improved, but also its mechanical properties can be enhanced; in addition, such introduction can also adjust the chemical properties of the epoxy resin so that it has specific functionality, such as flame retardancy and special reactivity, because the phenylboronic acid group has good flame retardancy.

[0010] Furthermore, the composite filler is obtained by mixing and reacting aluminum isopropoxide, ethyl acetoacetate, ethanol, modified boron nitride and a silane coupling agent.

[0011] Furthermore, the modified boron nitride is boron nitride modified by an aluminate coupling agent;

[0012] Furthermore, the silane coupling agent is heptadecafluorodecyltrimethoxysilane;

[0013] Furthermore, the aluminate coupling agent is isopropyl distearoyloxy aluminate;

[0014] Hexagonal boron nitride is a material with excellent thermal and chemical stability. Its layered structure is similar to that of graphite, but it has insulating properties. Hexagonal boron nitride is used to prepare composite fillers and mixed with modified epoxy resin to improve its thermal conductivity, wear resistance, mechanical properties, thermal stability, anti-aging properties and other properties.

[0015] The present invention also provides a method for preparing a powder coating for an electric drive system of a new energy vehicle, comprising the following preparation steps:

[0016] Add 50-80 parts by weight of modified epoxy resin to a sand mill dispersing and stirring multi-purpose machine, add 10% hydrochloric acid solution to a pH of 1, disperse at 2000-3000 r / min for 1 hour, then continue to drop 25% NaOH solution to a pH of 13, continue to disperse for 1 hour, let stand, remove the upper solution, then continue to add hydrochloric acid, 10% hydrochloric acid solution to a pH of 5, spin dry, add it together with 10-20 parts by weight of composite filler to a sand mill dispersing and stirring multi-purpose machine, heat up, and stir. To 80 ° C and disperse at 2000-3000 r / min for 8 hours, naturally cool to room temperature, add 2-4 parts by mass of curing agent, 0.2-0.8 parts by mass of imidazole accelerator, 1-2 parts by mass of leveling agent, 0.8 parts by mass of wax powder, 0.3-0.9 parts by mass of benzoin, 1-5 parts by mass of pigment, continue to disperse for 30 minutes, then put into a twin-screw extruder for extrusion, cool and crush, and then use a high-speed crusher to crush, pass through a 180-mesh standard sieve, and obtain a powder coating for the electric drive system of new energy vehicles.

[0017] Furthermore, the preparation method of the modified epoxy resin is as follows: under nitrogen protection and anhydrous conditions, 2-amino-4-hydroxy-6-methylpyrimidine and hexamethylene diisocyanate trimer are mixed in a molar ratio of 1:1, then heated to 60°C, vacuumed at a stirring speed of 150rpm until no bubbles are generated on the liquid surface, then heated to 90°C and stirred for reaction for 26 hours, cooled to room temperature, and then n-hexane with a mass of 20 to 40 times that of 2-amino-4-hydroxy-6-methylpyrimidine is added and stirred at room temperature for 4 to 6 hours, and then filtered with a sand core filter device, and the obtained filter residue is continuously washed with n-hexane, and the above operation is repeated until no hexamethylene diisocyanate remains in the filtrate, and then the filter residue is mixed with 4-aminophenylboronic acid pinacol ester and chloroform, wherein the molar ratio of hexamethylene diisocyanate trimer to 4-aminophenylboronic acid pinacol ester is 1:1, and the molar ratio of chloroform to The residues are mixed in a mass ratio of 1.7-1.9:15-16, stirred at 60°C for 12 hours, and then cooled to room temperature. The secondary residue is vacuum filtered with a sand core filter device to obtain a secondary residue. The secondary residue and chloroform are stirred and mixed at a mass ratio of 1:50-60, and then E51 epoxy resin is added. The molar ratio of hydroxyl in the epoxy resin to isocyanate in the secondary residue is 1:1-1.2. Dibutyltin dilaurate 0.1 times the mass of the secondary residue is added, and stirring and refluxing at 60°C for 24 hours is continued. Naturally cool to room temperature, chloroform 100 times the mass of the secondary residue is added to mix and dilute, and then stand for 12 hours. After taking out the lower layer solution, chloroform 150 times the mass of the secondary residue is added and stood for 24 hours. The lower layer solution is continued to be taken out. After repeating 5 times, the chloroform solvent is removed from the remaining solution by a rotary evaporator to obtain a modified epoxy resin.

[0018] Furthermore, the preparation method of the composite filler is as follows: at 25°C, aluminum isopropoxide, ethyl acetoacetate, and ethanol are ultrasonically mixed in a molar ratio of 1:1:5 for 10 minutes, poured into 85°C hot water 200 times the amount of aluminum isopropoxide at a speed of 250-300 r / min, the temperature and stirring rate are controlled unchanged, and after stirring for 30 minutes, 68% nitric acid is added to adjust the pH value to 3.2-3.5, and naturally cool to room temperature, and then 1.5 times the amount of isopropanol is added, and stirring is continued. Then, modified boron nitride and silane coupling agent are added in sequence, wherein the molar ratio of aluminum isopropoxide and silane coupling agent is 1:3, and the mass ratio of aluminum isopropoxide and modified boron nitride is 1:0.2-0.4, and stirring is continued for 2-4 hours to obtain a composite filler.

[0019] Furthermore, the preparation method of the modified boron nitride is as follows: hydroxylated boron nitride is added to a high-speed stirrer, stirred at 1500-2000 rpm for 20-40 min at 75° C., then an aluminate coupling agent is added, and stirring is continued for 2-4 h to obtain modified boron nitride.

[0020] Furthermore, the mass ratio of the aluminate coupling agent to hydroxylated boron nitride is 0.01-0.03:1.

[0021] Furthermore, the preparation method of the hydroxylated boron nitride is as follows: hexagonal boron nitride powder and sodium cholate powder are added to deionized water and mixed, wherein the mass ratio of hexagonal boron nitride powder, sodium cholate powder and deionized water is 1:0.01:40, and then placed in an ultrasonic cell crusher and treated with 600W ultrasound for 2.5 to 3.5 hours. After the ultrasound is completed, centrifuge it at a speed of 3000r / min for 8 to 12 minutes, and then remove the bottom precipitate, take the upper suspension, and dry it in an oven at 60°C to obtain hydroxylated boron nitride.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The powder coating for the electric drive system of a new energy vehicle prepared by the present invention comprises, by weight, raw material components: 50 to 80 parts of a composite epoxy resin, 10 to 20 parts of a composite filler, 2 to 4 parts of a curing agent, 0.2 to 0.8 parts of an imidazole accelerator, 1 to 2 parts of a leveling agent, 0.8 parts of wax powder, 0.3 to 0.9 parts of benzoin, and 1 to 5 parts of a pigment; the composite epoxy resin is obtained by a mixed reaction of 2-amino-4-hydroxy-6-methylpyrimidine, hexamethylene diisocyanate trimer, 4-aminophenylboronic acid pinacol ester, and an epoxy resin; the composite filler is obtained by a mixed reaction of aluminum isopropoxide, ethyl acetoacetate, ethanol, modified boron nitride, and a silane coupling agent; and the modified boron nitride is boron nitride modified by an aluminate coupling agent.

[0024] Firstly, modified boron nitride is prepared by reacting an aluminate coupling agent with hydroxylated boron nitride. After hydrolysis, the aluminate coupling agent reacts with the hydroxyl groups on the surface of boron nitride to form a condensation reaction and is coated on the surface of boron nitride. Subsequently, the modified boron nitride is uniformly dispersed in an alumina sol obtained by a mixed reaction of aluminum isopropoxide, ethyl acetoacetate and ethanol, thereby increasing the compatibility of boron nitride with the alumina sol. At the same time, heptadecafluorodecyltrimethoxysilane is added to the alumina sol to improve the hydrophobic properties of the composite filler, thereby improving the moisture and heat resistance of the powder coating for the electric drive system of new energy vehicles.

[0025] Secondly, the composite epoxy resin is obtained by a mixed reaction of 2-amino-4-hydroxy-6-methylpyrimidine, hexamethylene diisocyanate trimer, 4-aminophenylboronic acid pinacol ester, and epoxy resin. The amino groups on 2-amino-4-hydroxy-6-methylpyrimidine and 4-aminophenylboronic acid pinacol ester react with part of the isocyanate on the hexamethylene diisocyanate trimer, and the remaining isocyanate groups react with the hydroxyl groups in the epoxy resin to form a composite epoxy resin with a main chain containing an epoxy resin molecular chain side chain containing UPy groups, isocyanurate six-membered heterocyclic rings, and phenylboronic acid pinacol ester, thereby improving the composite epoxy resin. The toughness of epoxy resin is improved, wherein the UPy structure containing quadruple hydrogen bonds is introduced into the molecular chain of the composite epoxy resin, and the quadruple hydrogen bonds between the UPy groups act as physical cross-linking points, which is equivalent to "increasing" the cross-linking density of the composite epoxy resin; and during the stretching process of the composite epoxy resin, the breaking of the quadruple hydrogen bonds formed between the UPy groups consumes part of the energy, and the introduction of flexible side chains increases the sliding resistance between them, thereby enhancing the tensile strength and elongation at break of the composite epoxy resin, thereby enhancing the impact resistance of powder coatings for electric drive systems of new energy vehicles.

[0026] Finally, the composite epoxy resin and the composite filler are mixed. The -(CH2)16CH3 functional group on the isopropyl distearoyloxyaluminate in the composite filler is entangled with the molecular chain on the composite epoxy resin. In order to destroy the entangled structure, more heat needs to be absorbed, thereby ensuring the thermal stability of the powder coating for the electric drive system of new energy vehicles. The phenylboronic acid pinacol ester in the composite epoxy resin is hydrolyzed to obtain phenylboric acid, which reacts with the silanol in the composite filler to form polysiloxane, which firmly connects the composite epoxy resin and the composite filler. The Si-OBO segment in its molecular structure is a flexible segment, which is easy to undergo plastic deformation when subjected to external force, thereby enhancing the thermal stability of the powder coating. The slip ability between molecular chains is improved, which is manifested as a higher elongation at break of the material on a macroscopic level; in addition, the Si-OBO structure in the PBSi molecular structure provides good thermal stability; at the same time, the hydrophobic Si-O bond contained in PBSi has a lower surface energy than the CH bond, which helps to reduce the surface energy of the PLA film and reduce the contact area between it and water, thereby increasing the interfacial energy between the two and turning the material into hydrophobic, thereby further enhancing the impact resistance and moisture and heat resistance of the insulating anti-aging powder coating; at the same time, polysiloxane forms a thermal conductive network with the boron nitride in the composite filler, which enhances the thermal conductivity of the composite epoxy resin. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with examples, but the following examples should not be construed as limiting the present invention.

[0028] Some of the raw materials of the embodiments of the present invention and the comparative examples are as follows:

[0029] The epoxy resin is E51 epoxy resin, the average epoxy value of which is 0.51 and the average hydroxyl value of which is 0.046.

[0030] Example 1

[0031] A method for preparing a powder coating for an electric drive system of a new energy vehicle, the preparation steps are as follows:

[0032] 50 parts by mass of modified epoxy resin are added to a sand mill dispersing and stirring multi-purpose machine, 10% hydrochloric acid solution is added to pH 1, and the mixture is dispersed at 2000 r / min for 1 hour, and then a 25% NaOH solution is continuously added dropwise to a pH value of 13, and the mixture is dispersed for 1 hour. The mixture is allowed to stand and the upper solution is removed. Then, hydrochloric acid is continuously added to a 10% hydrochloric acid solution to a pH value of 5. After being spun dry, the mixture is added to a sand mill dispersing and stirring multi-purpose machine together with 10 parts by mass of a composite filler, the mixture is heated to 80° C. and dispersed at 2000 r / min for 8 hours. After naturally cooling to room temperature, 2 parts by mass of a curing agent, 0.2 parts by mass of an imidazole accelerator, 1 part by mass of a leveling agent, 0.8 parts by mass of wax powder, 0.3 parts by mass of benzoin, and 1 part by mass of a pigment are added, and the mixture is dispersed for 30 minutes. The mixture is then extruded by a twin-screw extruder, cooled and crushed, and then crushed with a high-speed crusher, and passed through a 180-mesh standard sieve to obtain a powder coating for an electric drive system of a new energy vehicle.

[0033] The preparation method of the modified epoxy resin is as follows: under nitrogen protection and anhydrous conditions, 2-amino-4-hydroxy-6-methylpyrimidine and hexamethylene diisocyanate trimer are mixed in a molar ratio of 1:1, then heated to 60°C, vacuumed at a stirring speed of 150rpm until no bubbles are generated on the liquid surface, then heated to 90°C and stirred for reaction for 26h, cooled to room temperature, added with n-hexane 20 times the mass of 2-amino-4-hydroxy-6-methylpyrimidine, stirred at room temperature for 4h, and then filtered with a sand core filter device, the obtained filter residue is continuously washed with n-hexane, the above operation is repeated until no hexamethylene diisocyanate remains in the filtrate, and then the filter residue is mixed with 4-aminophenylboronic acid pinacol ester and chloroform, wherein the molar ratio of hexamethylene diisocyanate trimer to 4-aminophenylboronic acid pinacol ester is 1:1, and the chloroform is 1:2. The imitation and filter residue are mixed in a mass ratio of 1.7:15, stirred at 60°C for 12h, and continued to cool to room temperature, and then vacuum filtered with a sand core filter device to obtain a secondary filter residue. The secondary filter residue and chloroform are stirred and mixed at a mass ratio of 1:50, and then E51 epoxy resin is added. The molar ratio of hydroxyl in the epoxy resin to isocyanate in the secondary filter residue is 1:1. Dibutyltin dilaurate 0.1 times the mass of the secondary filter residue is added, and stirring and refluxing at 60°C for 24h is continued. Naturally cool to room temperature, chloroform 100 times the mass of the secondary filter residue is added to dilute the mixture and let it stand for 12h. After taking out the lower layer solution, chloroform 150 times the mass of the secondary filter residue is added and let it stand for 24h. The lower layer solution is continued to be taken out. After repeating 5 times, the chloroform solvent is removed from the remaining solution by a rotary evaporator to obtain a modified epoxy resin.

[0034] The preparation method of the composite filler is as follows: at 25°C, aluminum isopropoxide, ethyl acetoacetate, and ethanol are ultrasonically mixed in a molar ratio of 1:1:5 for 10 minutes, poured into 85°C hot water with a volume of 200 times the volume of the aluminum isopropoxide substance at a speed of 250 r / min, the temperature and stirring rate are kept constant, and after stirring for 30 minutes, nitric acid with a concentration of 68% is added to adjust the pH value to 3.2, and naturally cool to room temperature, and then isopropanol with a volume of 1.5 times the volume of the aluminum isopropoxide substance is added, and stirring is continued, and then modified boron nitride and silane coupling agent are added in sequence, wherein the molar ratio of aluminum isopropoxide to the silane coupling agent is 1:3, and the mass ratio of aluminum isopropoxide to the modified boron nitride is 1:0.2, and stirring is continued for 2 hours to obtain the composite filler.

[0035] The preparation method of the modified boron nitride is as follows: hydroxylated boron nitride is added to a high-speed stirrer, stirred at 1500 rpm for 20 minutes at 75° C., then an aluminate coupling agent is added, and stirring is continued for 2 hours to obtain modified boron nitride.

[0036] The mass ratio of the aluminate coupling agent to the hydroxylated boron nitride is 0.01:1.

[0037] The preparation method of the hydroxylated boron nitride is as follows: hexagonal boron nitride powder and sodium cholate powder are added into deionized water and mixed, wherein the mass ratio of the hexagonal boron nitride powder, the sodium cholate powder and the deionized water is 1:0.01:40, and then the mixture is placed into an ultrasonic cell crusher and subjected to 600W ultrasonic treatment for 2.5 hours. After the ultrasonic treatment, the mixture is centrifuged at a speed of 3000r / min for 8 minutes in a centrifuge, and then the bottom precipitate is removed, and the upper suspension is taken and dried in an oven at 60°C to obtain hydroxylated boron nitride.

[0038] Example 2

[0039] A method for preparing a powder coating for an electric drive system of a new energy vehicle, the preparation steps are as follows:

[0040] 65 parts by mass of modified epoxy resin are added to a sand mill dispersing and stirring multi-purpose machine, 10% hydrochloric acid solution is added to pH 1, and the mixture is dispersed at 2500 r / min for 1 hour, and then a 25% NaOH solution is continuously added dropwise to a pH value of 13, and the mixture is dispersed for 1 hour. The mixture is allowed to stand and the upper solution is removed. Then, hydrochloric acid is continuously added to a 10% hydrochloric acid solution to a pH value of 5. After being spun dry, the mixture is added to a sand mill dispersing and stirring multi-purpose machine together with 15 parts by mass of composite fillers, and the mixture is heated to 80° C. and dispersed at 2500 r / min for 8 hours. After naturally cooling to room temperature, 3 parts by mass of curing agent, 0.5 parts by mass of imidazole accelerator, 1.5 parts by mass of leveling agent, 0.8 parts by mass of wax powder, 0.6 parts by mass of benzoin, and 3 parts by mass of pigment are added, and the mixture is dispersed for 30 minutes. The mixture is then put into a twin-screw extruder for extrusion, cooled and crushed, and then crushed with a high-speed crusher, and passed through a 180-mesh standard sieve to obtain a powder coating for an electric drive system of a new energy vehicle.

[0041] The preparation method of the modified epoxy resin is as follows: under nitrogen protection and anhydrous conditions, 2-amino-4-hydroxy-6-methylpyrimidine and hexamethylene diisocyanate trimer are mixed in a molar ratio of 1:1, then heated to 60°C, vacuumed at a stirring speed of 150rpm until no bubbles are generated on the liquid surface, then heated to 90°C and stirred for reaction for 26 hours, cooled to room temperature, added with n-hexane 30 times the mass of 2-amino-4-hydroxy-6-methylpyrimidine, stirred at room temperature for 5 hours, and then filtered with a sand core filter device, the obtained filter residue is continuously washed with n-hexane, and the above operation is repeated until no hexamethylene diisocyanate remains in the filtrate, and then the filter residue is mixed with 4-aminophenylboronic acid pinacol ester and chloroform, wherein the molar ratio of hexamethylene diisocyanate trimer to 4-aminophenylboronic acid pinacol ester is 1:1, and the molar ratio of chloroform to The residues were mixed in a mass ratio of 1.8:15.5, stirred at 60°C for 12 hours, and continued to cool to room temperature. The secondary residue was vacuum filtered with a sand core filter device to obtain a secondary residue. The secondary residue and chloroform were stirred and mixed at a mass ratio of 1:55. Then E51 epoxy resin was added. The molar ratio of hydroxyl in the epoxy resin to isocyanate in the secondary residue was 1:1.1. Dibutyltin dilaurate was added in an amount of 0.1 times the mass of the secondary residue. The mixture was stirred and refluxed at 60°C for 24 hours. The mixture was naturally cooled to room temperature. Chloroform was added in an amount of 100 times the mass of the secondary residue to mix and dilute the mixture, and then allowed to stand for 12 hours. The lower solution was taken out and chloroform was added in an amount of 150 times the mass of the secondary residue to stand for 24 hours. The lower solution was continued to be taken out. After repeating 5 times, the chloroform solvent was removed from the remaining solution by a rotary evaporator to obtain a modified epoxy resin.

[0042] The preparation method of the composite filler is as follows: at 25°C, aluminum isopropoxide, ethyl acetoacetate, and ethanol are ultrasonically mixed in a molar ratio of 1:1:5 for 10 minutes, poured into 85°C hot water with a volume of 200 times the volume of the aluminum isopropoxide substance at a speed of 280 r / min, the temperature and stirring rate are kept constant, and after stirring for 30 minutes, nitric acid with a concentration of 68% is added to adjust the pH value to 3.3, and naturally cool to room temperature, and then isopropanol with a volume of 1.5 times the volume of the aluminum isopropoxide substance is added, and stirring is continued, and then modified boron nitride and silane coupling agent are added in sequence, wherein the molar ratio of aluminum isopropoxide to the silane coupling agent is 1:3, and the mass ratio of aluminum isopropoxide to the modified boron nitride is 1:0.3, and stirring is continued for 3 hours to obtain the composite filler.

[0043] The preparation method of the modified boron nitride is as follows: hydroxylated boron nitride is added to a high-speed stirrer, stirred at 1800 rpm for 30 minutes at 75° C., then an aluminate coupling agent is added, and stirring is continued for 3 hours to obtain modified boron nitride.

[0044] The mass ratio of the aluminate coupling agent to the hydroxylated boron nitride is 0.02:1.

[0045] The preparation method of the hydroxylated boron nitride is as follows: hexagonal boron nitride powder and sodium cholate powder are added into deionized water and mixed, wherein the mass ratio of the hexagonal boron nitride powder, the sodium cholate powder and the deionized water is 1:0.01:40, and then the mixture is placed in an ultrasonic cell crusher and subjected to 600W ultrasonic treatment for 3 hours. After the ultrasonic treatment, the mixture is centrifuged at a speed of 3000r / min for 10 minutes in a centrifuge, and then the bottom precipitate is removed, and the upper suspension is taken and dried in an oven at 60°C to obtain hydroxylated boron nitride.

[0046] Example 3

[0047] A method for preparing a powder coating for an electric drive system of a new energy vehicle, the preparation steps are as follows:

[0048] 80 parts by weight of modified epoxy resin are added to a sand mill dispersing and stirring multi-purpose machine, 10% hydrochloric acid solution is added to a pH of 1, and the mixture is dispersed at 3000 r / min for 1 hour, and then a 25% NaOH solution is continuously added dropwise to a pH of 13, and the mixture is dispersed for 1 hour. The mixture is allowed to stand and the upper solution is removed. Then, hydrochloric acid is continuously added to a 10% hydrochloric acid solution to a pH of 5, and the mixture is spin-dried and added to a sand mill dispersing and stirring multi-purpose machine together with 20 parts by weight of composite fillers, and the mixture is heated to 80° C. and dispersed at 3000 r / min for 8 hours. After naturally cooling to room temperature, 4 parts by weight of curing agent, 0.8 parts by weight of imidazole accelerator, 2 parts by weight of leveling agent, 0.8 parts by weight of wax powder, 0.9 parts by weight of benzoin, and 5 parts by weight of pigment are added, and the mixture is dispersed for 30 minutes. The mixture is then put into a twin-screw extruder for extrusion, cooled and crushed, and then crushed with a high-speed crusher, and passed through a 180-mesh standard sieve to obtain a powder coating for an electric drive system of a new energy vehicle.

[0049] The preparation method of the modified epoxy resin is as follows: under nitrogen protection and anhydrous conditions, 2-amino-4-hydroxy-6-methylpyrimidine and hexamethylene diisocyanate trimer are mixed in a molar ratio of 1:1, then heated to 60°C, vacuumed at a stirring speed of 150rpm until no bubbles are generated on the liquid surface, then heated to 90°C and stirred for reaction for 26 hours, cooled to room temperature, added with n-hexane 40 times the mass of 2-amino-4-hydroxy-6-methylpyrimidine, stirred at room temperature for 6 hours, and then filtered with a sand core filter device, the obtained filter residue is continuously washed with n-hexane, and the above operation is repeated until no hexamethylene diisocyanate remains in the filtrate, and then the filter residue is mixed with 4-aminophenylboronic acid pinacol ester and chloroform, wherein the molar ratio of hexamethylene diisocyanate trimer to 4-aminophenylboronic acid pinacol ester is 1:1, and the chloroform is 1:2. The mixture was mixed with the filter residue in a mass ratio of 1.9:16, stirred at 60°C for 12 hours, and then cooled to room temperature, and then vacuum filtered with a sand core filter device to obtain a secondary filter residue. The secondary filter residue and chloroform were stirred and evenly mixed in a mass ratio of 1:60, and then E51 epoxy resin was added, the molar ratio of hydroxyl in the epoxy resin to isocyanate in the secondary filter residue was 1:1.2, and dibutyltin dilaurate was added in an amount of 0.1 times the mass of the secondary filter residue, and stirring and refluxing were continued at 60°C for 24 hours. The mixture was naturally cooled to room temperature, and chloroform was added in an amount of 100 times the mass of the secondary filter residue to mix and dilute, and then allowed to stand for 12 hours. The lower layer solution was taken out, and then chloroform was added in an amount of 150 times the mass of the secondary filter residue and allowed to stand for 24 hours. The lower layer solution was continued to be taken out, and after repeating 5 times, the chloroform solvent was removed from the remaining solution by a rotary evaporator to obtain a modified epoxy resin.

[0050] The preparation method of the composite filler is as follows: at 25°C, aluminum isopropoxide, ethyl acetoacetate, and ethanol are ultrasonically mixed in a molar ratio of 1:1:5 for 10 minutes, poured into 85°C hot water with a volume of 200 times the volume of the aluminum isopropoxide substance at a speed of 300 r / min, the temperature and stirring rate are kept constant, and after stirring for 30 minutes, nitric acid with a concentration of 68% is added to adjust the pH value to 3.5, and naturally cool to room temperature, and then isopropanol with a volume of 1.5 times the volume of the aluminum isopropoxide substance is added, and stirring is continued, and then modified boron nitride and silane coupling agent are added in sequence, wherein the molar ratio of aluminum isopropoxide to silane coupling agent is 1:3, and the mass ratio of aluminum isopropoxide to modified boron nitride is 1:0.4, and stirring is continued for 4 hours to obtain the composite filler.

[0051] The preparation method of the modified boron nitride is as follows: hydroxylated boron nitride is added to a high-speed stirrer, stirred at 2000 rpm for 40 minutes at 75° C., then an aluminate coupling agent is added, and stirring is continued for 4 hours to obtain modified boron nitride.

[0052] The mass ratio of the aluminate coupling agent to the hydroxylated boron nitride is 0.03:1.

[0053] The preparation method of the hydroxylated boron nitride is as follows: hexagonal boron nitride powder and sodium cholate powder are added into deionized water and mixed, wherein the mass ratio of the hexagonal boron nitride powder, the sodium cholate powder and the deionized water is 1:0.01:40, and then the mixture is placed into an ultrasonic cell crusher and subjected to 600W ultrasonic treatment for 3.5 hours. After the ultrasonic treatment, the mixture is centrifuged at a speed of 3000r / min for 12 minutes in a centrifuge, and then the bottom precipitate is removed, and the upper suspension is taken and dried in an oven at 60°C to obtain hydroxylated boron nitride.

[0054] Comparative Example 1

[0055] The only difference between Comparative Example 1 and Example 2 is that the composite epoxy resin is obtained by mixing and reacting hexamethylene diisocyanate trimer, 4-aminophenylboronic acid pinacol ester, and epoxy resin, and the remaining steps and ingredients are the same as those in Example 2.

[0056] Comparative Example 2

[0057] The difference between Comparative Example 2 and Example 2 is that the composite epoxy resin is obtained by mixing 2-amino-4-hydroxy-6-methylpyrimidine, hexamethylene diisocyanate, 4-aminophenylboronic acid pinacol ester, and epoxy resin; the remaining steps and components are the same as those in Example 2.

[0058] Comparative Example 3

[0059] The only difference between Comparative Example 3 and Example 2 is that the composite epoxy resin is obtained by mixing 2-amino-4-hydroxy-6-methylpyrimidine, hexamethylene diisocyanate trimer and epoxy resin, and the remaining steps and ingredients are the same as those in Example 2.

[0060] Comparative Example 4

[0061] The only difference between Comparative Example 4 and Example 2 is that epoxy resin is used to prepare the powder coating for the electric drive system of new energy vehicles; the remaining steps and ingredients are the same as those in Example 2.

[0062] Comparative Example 5

[0063] The difference between Comparative Example 5 and Example 2 is that the composite filler is obtained by mixing and reacting aluminum isopropoxide, ethyl acetoacetate, ethanol, boron nitride, and a silane coupling agent; the remaining steps and ingredients are the same as those in Example 2.

[0064] Comparative Example 6

[0065] The only difference between Comparative Example 6 and Example 2 is that the composite filler is obtained by mixing aluminum isopropoxide, ethyl acetoacetate, ethanol, and modified boron nitride; the remaining steps and ingredients are the same as those in Example 2.

[0066] Comparative Example 7

[0067] The difference between Comparative Example 7 and Example 2 is that the composite filler is obtained by mixing modified boron nitride and a silane coupling agent; the remaining steps and components are the same as those in Example 2.

[0068] Comparative Example 8

[0069] The only difference between Comparative Example 8 and Example 2 is that boron nitride is used to prepare the powder coating for the electric drive system of new energy vehicles; the remaining steps and ingredients are the same as those in Example 2.

[0070] Effect example

[0071] Table 1 below shows the performance test standards and evaluation indicators of powder coatings for electric drive systems of new energy vehicles:

[0072] Table 1

[0073]

[0074] Table 2 below shows the performance test analysis results of the powder coatings for electric drive systems of new energy vehicles prepared by Examples 1 to 3 of the present invention and Comparative Examples 1 to 8.

[0075] Table 1

[0076]

[0077] From Table 1, it can be found that the insulation, impact resistance, moisture and heat resistance, thermal stability, flame retardancy and hardness of the powder coating for the electric drive system of new energy vehicles prepared in the embodiment are good; compared with Comparative Examples 1, 2, 3 and 4, Example 2 shows that the composite epoxy resin obtained by the mixed reaction of 2-amino-4-hydroxy-6-methylpyrimidine, hexamethylene diisocyanate trimer, 4-aminophenylboronic acid pinacol ester and epoxy resin is used to prepare the powder coating for the electric drive system of new energy vehicles, and the obtained powder coating for the electric drive system of new energy vehicles has good insulation, impact resistance, moisture and heat resistance, thermal stability, flame retardancy and hardness; compared with Comparative Examples 5, 6, 7 and 8, Example 2 shows that the composite filler obtained by the mixed reaction of aluminum isopropoxide, ethyl acetoacetate, ethanol, modified boron nitride and silane coupling agent is used to prepare the powder coating for the electric drive system of new energy vehicles, and the obtained powder coating for the electric drive system of new energy vehicles has good insulation, impact resistance, moisture and heat resistance, thermal stability, flame retardancy and hardness.

[0078] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A powder coating for electric drive system of new energy vehicles, characterized in that: The raw material components include, by weight: 50 to 80 parts of composite epoxy resin, 10 to 20 parts of composite filler, 2 to 4 parts of curing agent, 0.2 to 0.8 parts of imidazole accelerator, 1 to 2 parts of leveling agent, 0.8 parts of wax powder, 0.3 to 0.9 parts of benzoin, and 1 to 5 parts of pigment.

2. The powder coating for the electric drive system of new energy vehicles according to claim 1, characterized in that: The composite epoxy resin is obtained by a mixed reaction of 2-amino-4-hydroxy-6-methylpyrimidine, hexamethylene diisocyanate trimer, 4-aminophenylboronic acid pinacol ester and epoxy resin.

3. The powder coating for the electric drive system of new energy vehicles according to claim 1, characterized in that: The composite filler is obtained by mixing and reacting aluminum isopropoxide, ethyl acetoacetate, ethanol, modified boron nitride and a silane coupling agent.

4. The powder coating for the electric drive system of new energy vehicles according to claim 3, characterized in that: The modified boron nitride is boron nitride modified by an aluminate coupling agent.

5. A method for preparing a powder coating for a new energy vehicle electric drive system according to any one of claims 1 to 4, characterized in that: The method comprises the following preparation steps: Add 50-80 parts by weight of modified epoxy resin to a sand mill dispersing and stirring multi-purpose machine, add 10% hydrochloric acid solution to a pH of 1, disperse at 2000-3000 r / min for 1 hour, then continue to drop 25% NaOH solution to a pH of 13, continue to disperse for 1 hour, let stand, remove the upper solution, then continue to add hydrochloric acid, 10% hydrochloric acid solution to a pH of 5, spin dry, add it together with 10-20 parts by weight of composite filler to a sand mill dispersing and stirring multi-purpose machine, heat up, and stir. To 80 ° C and disperse at 2000-3000 r / min for 8 hours, naturally cool to room temperature, add 2-4 parts by mass of curing agent, 0.2-0.8 parts by mass of imidazole accelerator, 1-2 parts by mass of leveling agent, 0.8 parts by mass of wax powder, 0.3-0.9 parts by mass of benzoin, 1-5 parts by mass of pigment, continue to disperse for 30 minutes, then put into a twin-screw extruder for extrusion, cool and crush, and then use a high-speed crusher to crush, pass through a 180-mesh standard sieve, and obtain a powder coating for the electric drive system of new energy vehicles.

6. The method for preparing powder coating for electric drive system of new energy vehicle according to claim 5, characterized in that: The preparation method of the modified epoxy resin is as follows: under nitrogen protection and anhydrous conditions, 2-amino-4-hydroxy-6-methylpyrimidine and hexamethylene diisocyanate trimer are mixed in a molar ratio of 1:1, then heated to 60°C, vacuumed at a stirring speed of 150rpm until no bubbles are generated on the liquid surface, then heated to 90°C and stirred for reaction for 26 hours, cooled to room temperature, added with n-hexane 20 to 40 times the mass of 2-amino-4-hydroxy-6-methylpyrimidine, stirred at room temperature for 4 to 6 hours, and then filtered with a sand core filter device, the obtained filter residue is continuously washed with n-hexane, and the above operation is repeated until no hexamethylene diisocyanate remains in the filtrate, and then the filter residue is mixed with 4-aminophenylboronic acid pinacol ester and chloroform, wherein the molar ratio of hexamethylene diisocyanate trimer to 4-aminophenylboronic acid pinacol ester is 1:1, and the molar ratio of chloroform to the filter residue is 1:

1. The mixture was mixed at a mass ratio of 1.7-1.9:15-16, stirred at 60°C for 12h, and then cooled to room temperature. The secondary filter residue and chloroform were vacuum filtered with a sand core filter device to obtain a secondary filter residue. The secondary filter residue and chloroform were mixed at a mass ratio of 1:50-60, and then E51 epoxy resin was added. The molar ratio of hydroxyl in the epoxy resin to isocyanate in the secondary filter residue was 1:1-1.

2. Dibutyltin dilaurate was added at a mass of 0.1 times the mass of the secondary filter residue, and the mixture was stirred and refluxed at 60°C for 24h. The mixture was naturally cooled to room temperature, and chloroform was added at a mass of 100 times the mass of the secondary filter residue to mix and dilute, and then the mixture was allowed to stand for 12h. The lower layer solution was taken out, and then chloroform was added at a mass of 150 times the mass of the secondary filter residue to stand for 24h. The lower layer solution was taken out, and the chloroform solvent was removed from the remaining solution by a rotary evaporator after repeating 5 times to obtain a modified epoxy resin.

7. The method for preparing powder coating for electric drive system of new energy vehicle according to claim 5, characterized in that: The preparation method of the composite filler is as follows: at 25°C, aluminum isopropoxide, ethyl acetoacetate and ethanol are ultrasonically mixed in a molar ratio of 1:1:5 for 10 minutes, poured into 85°C hot water with a volume of 200 times the volume of the aluminum isopropoxide substance at a speed of 250-300 r / min, the temperature and stirring rate are kept constant, after stirring for 30 minutes, a pH value is adjusted to 3.2-3.5 by adding 68% of the concentration of aluminum isopropoxide, naturally cooled to room temperature, then isopropanol with a volume of 1.5 times the volume of the aluminum isopropoxide substance is added, stirring is continued, and then modified boron nitride and silane coupling agent are added in sequence, wherein the molar ratio of aluminum isopropoxide to the silane coupling agent is 1:3, and the mass ratio of aluminum isopropoxide to the modified boron nitride is 1:0.2-0.4, stirring is continued for 2-4 hours, and the composite filler is obtained.

8. The method for preparing powder coating for electric drive system of new energy vehicle according to claim 7, characterized in that: The preparation method of the modified boron nitride is as follows: hydroxylated boron nitride is added to a high-speed stirrer, stirred at 75°C at 1500-2000 rpm for 20-40 minutes, then an aluminate coupling agent is added, and stirring is continued for 2-4 hours to obtain modified boron nitride.

9. The method for preparing powder coating for electric drive system of new energy vehicle according to claim 8, characterized in that: The mass ratio of the aluminate coupling agent to the hydroxylated boron nitride is 0.01-0.03:

1.

10. The method for preparing powder coating for electric drive system of new energy vehicle according to claim 8, characterized in that: The preparation method of the hydroxylated boron nitride is as follows: hexagonal boron nitride powder and sodium cholate powder are added into deionized water and mixed, wherein the mass ratio of the hexagonal boron nitride powder, the sodium cholate powder and the deionized water is 1:0.01:40, and then the mixture is put into an ultrasonic cell crusher and subjected to 600W ultrasonic treatment for 2.5 to 3.5 hours. After the ultrasonic treatment, the mixture is centrifuged at a speed of 3000 r / min for 8 to 12 minutes in a centrifuge, and then the bottom precipitate is removed, and the upper suspension is taken and dried in an oven at 60°C to obtain hydroxylated boron nitride.

Citation Information

Patent Citations

  • Method for preparing photic driving self-repair film based on ethylene-butylene copolymer

    CN106221100A

  • Preparation method of epoxy resin composite material based on quadruple hydrogen bond supermolecular self repairing

    CN108715667A

  • Thermosetting epoxy resin composite material, preparation method and recovery method thereof, recovered thermosetting epoxy resin composite material and application thereof

    CN116444948A

  • Aluminate coupling agent as well as preparation method and application thereof

    CN118580692A

  • Poudery coating composition

    EP0000971A1

Cited By

  • Flame-retardant high-wear-resistance epoxy powder coating and preparation method thereof

    CN119955374A

  • A flame retardant and highly wear-resistant epoxy powder coating and its preparation method

    CN119955374B

  • High-performance water-based phenoxy resin coating as well as preparation method and application thereof

    CN120682706A

  • High performance waterborne phenoxy resin coating and its preparation method and application

    CN120682706B

  • Insulating spraying composite material for power transmission and transformation system and preparation method of insulating spraying composite material

    CN120818283A