A method for synthesizing supramolecular cross-linked polymers of pillared aromatics and terpyridine
By using model compounds and Zn(OTf)2 in CDCl3 and DMSO-d6 solvents to achieve complementary metal coordination reactions of terpyridine metal complexes, pillararenes and terpyridine supramolecular cross-linked polymers were constructed, solving the existing technical problems The problems of single performance and high cost of terpyridine metal complexes have been solved, and simplified synthesis and large-scale production have been achieved.
Patent Information
- Application Number
- CN202311220678.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-09-21
AI Technical Summary
Existing terpyridine metal complexes have single properties, unfriendly reaction conditions, high synthesis costs, and difficulty in solution processing. There are no reports on the construction of supramolecular cross-linking of pillararenes and terpyridine to form new polymers.
Through the orthogonal non-covalent interaction of model compounds M1, M2, M3 and Zn(OTf)2 in CDCl3, DMSO-d6 mixed solvent, the complementary metal coordination of monomers A4, B4, M1 and Zn(OTf)2 is realized. Site interactions and host-guest reactions build supramolecular cross-linked polymers of pillararenes and terpyridine.
The preparation method is simplified, the reaction conditions are mild, the synthesis cost is reduced, it is conducive to large-scale production, and a new material with supramolecular polymer gel is formed.
Smart Images

Figure CN117050331B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemistry, and in particular relates to a method for synthesizing a pillared aromatic hydrocarbon and terpyridine supramolecular cross-linked polymer. Background Art
[0002] Currently, the most reported are metal polymer materials based on terpyridine ligands. Terpyridine is a good tridentate ligand. The whole system forms a large conjugated system with strong electron donating ability. When the terpyridine ligand is coordinated with the metal, there is a metal-to-ligand bonding effect. The terpyridine ligand can react with some transition metal ions to obtain metal polymer materials based on terpyridine ligands.
[0003] Common terpyridine-based metal complexes in the prior art include terpyridine ruthenium (II) complexes, terpyridine iron (II) complexes, terpyridine platinum (II) complexes, terpyridine gold (II) complexes, etc. There are no reports on the synthesis and application of new polymers formed by cross-linking pillared aromatics and terpyridine supramolecular molecules.
[0004] Moreover, the above-mentioned existing terpyridine metal complexes have single performance, unfriendly reaction conditions, relatively high synthesis costs, and the complexes are usually not easy to process in solution. In view of the above factors, a method for constructing a columnar aromatic hydrocarbon and terpyridine supramolecular cross-linked polymer is provided. A new polymer is formed by cross-linking columnar aromatic hydrocarbons and terpyridine supramolecular cross-linking. The preparation method is simple, the reaction conditions are mild, the synthesis cost is relatively low, and it is conducive to large-scale production. Summary of the invention
[0005] The object of the present invention is to provide a method for synthesizing a supramolecular cross-linked polymer of pillared aromatics and terpyridine to solve the problems raised in the above background technology.
[0006] The objective of the present invention is achieved through the following technical scheme: a method for synthesizing supramolecular cross-linked polymers of pillar aromatics and terpyridines, wherein the orthogonal non-covalent interactions of model compounds M1, M2, M3 and Zn(OTf)2 in a mixed solvent of CDCl3 and DMSO-d6 enable the orthogonal self-assembly of monomers A4, B4, M1 and Zn(OTf)2 through complementary metal coordination interactions and host-guest reactions to form supramolecular cross-linked polymers of pillar aromatics and terpyridines.
[0007] A method for synthesizing a pillared aromatic hydrocarbon and terpyridine supramolecular cross-linked polymer comprises the following steps:
[0008] In an air atmosphere, 10 mmol A4, 10 mmol B4, 40 mmol M1 and 40 mmol Zn(OTf)2 were dissolved in a mixed solvent of CDCl3 and DMSO-d6, and the non-covalent interaction between A4, B4, M1 and Zn(OTf)2 was monitored by hydrogen nuclear magnetic resonance spectroscopy until the complexation was complete.
[0009] The preparation method of monomer B4 comprises the following steps:
[0010] 0.1 g, 0.39 mmol and 50 ml SOCl2 of 1,2,4,5-benzenetetracarboxylic acid were added to a round-bottom flask, 0.3 ml DMF was added dropwise, and the mixture was stirred and refluxed at 80 degrees Celsius for 8 hours. The mixture was cooled and the solvent was removed by spin-drying under reduced pressure to obtain an oily liquid, which was dissolved in 10 ml dry THF and slowly added dropwise to a round-bottom flask containing 0.75 g, 1.60 mmol, 0.2 ml Et3N and 40 ml dry THF of compound 5 at 0 degrees Celsius. After the addition was completed, the mixture was stirred at 0 degrees Celsius for 12 hours, and then reacted at 25 degrees Celsius for 12 hours. The initial reaction product was extracted with dichloromethane and water, dried over anhydrous sodium sulfate, and the solvent was removed by spin-drying under reduced pressure. The crude product was purified by column chromatography to obtain monomer B4 as a white solid.
[0011] Furthermore, the ratio of the CDCl3:DMSO-d6 mixed solvent is 5:1.
[0012] Furthermore, the terpyridine group in monomer B4 and the 9-anthryl terpyridine group in monomer M1 are reacted by Zn 2+ The effect of the two metals forms a stable complementary metal coordination structure.
[0013] Furthermore, the terpyridine group substituted by the 9-anthryl group on the monomer M1 undergoes metal coordination with the terpyridine group on the monomer M2 to form a stable complementary metal complex tey-Zn 2+ -tpy;
[0014] The monomers B4 and M1 and the monomers M1 and the model compound M2 form the same stable complementary metal complex tey-Zn 2+ -tpy.
[0015] Further, the chemical structure of the M1 monomer is as follows;
[0016]
[0017] Further, the chemical structure of the B4 monomer is as follows;
[0018]
[0019] Further, the chemical structure of the A4 monomer is as follows;
[0020]
[0021] A gel prepared by a synthetic method of constructing a supramolecular cross-linked polymer of pillar aromatics and terpyridine. In an air atmosphere, A4, B4, M1 and Zn(OTf)2 are mixed in a ratio of 1:1:4:4. When the concentration of the monomer M1 exceeds 60 mM, the supramolecular cross-linked polymer forms a supramolecular polymer gel.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention adopts monomer A4+B4+M1+Zn 2+ Hybrid, self-assembly to form supramolecular polymers based on complementary metal coordination interactions and host-guest reactions.
[0024] The invention provides a method for synthesizing a pillared aromatic hydrocarbon and terpyridine supramolecular cross-linked polymer. The preparation method is simple, the preparation method is simplified, the reaction conditions are mild, the synthesis cost is relatively reduced, and large-scale production is facilitated. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic diagram of the construction of supramolecular cross-linked polymers based on pillar aromatics and terpyridine in the present invention.
[0026] Figure 2 is the hydrogen nuclear magnetic resonance spectrum of monomer A4 of the present invention;
[0027] Figure 3 is the carbon NMR spectrum of monomer A4 of the present invention;
[0028] Figure 4 is the matrix-assisted time-of-flight mass spectrometry of monomer A4 of the present invention;
[0029] Figure 5 is the hydrogen nuclear magnetic resonance spectrum of monomer B4 of the present invention;
[0030] Figure 6 is the carbon NMR spectrum of monomer B4 of the present invention;
[0031] Figure 7 is the high-resolution mass spectrum of monomer B4 of the present invention;
[0032] Figure 8 is the hydrogen nuclear magnetic resonance spectrum of the monomer M1 of the present invention;
[0033] Fig. 9The following are hydrogen nuclear magnetic resonance spectra (400 MHz, CDCl3:DMSO-d6=5:1) of the model compounds M1 and M3 of the present invention: (a) M1; (b) M1+M3; (c) M3;
[0034] Fig.10 The following are hydrogen nuclear magnetic resonance spectra of M1, M2 and Zn(OTf)2 of the present invention (400 MHz, CDCl3:DMSO-d6=5:1): (a) M2; (b) M1+M2+Zn(OTf)2; (c) M1;
[0035] Fig.11 The following are hydrogen nuclear magnetic resonance spectra of the model compounds M1, M2, M3 and Zn(OTf)2 of the present invention (400 MHz, CDCl3:DMSO-d6=5:1): (a) M2+M3+Zn(OTf)2; (b) M1+M2+M3+Zn(OTf)2; (c) M1+M3;
[0036] Fig.12 The following are hydrogen nuclear magnetic resonance spectra of monomers A4, B4, M1 and Zn(OTf)2 of the present invention (400 MHz, CDCl3:DMSO-d6=5:1): (a) M1+A4+B4+Zn(OTf)2; (b) A4; (c) M1; (d) B4; the proton signal of the monomer after coordination is marked with subscript c;
[0037] Fig.13 The concentration-dependent H NMR spectrum of M1+A4+B4+Zn(OTf)2 of the present invention (400 MHz, CDCl3:DMSO-d6=5:1, A4:B:M1:Zn(OTf)2=1:1:4:4): (a) the concentration of M1 is 64 mM, (b) the concentration of M1 is 32 mM, (c) the concentration of M1 is 16 mM, (d) the concentration of M1 is 8 mM, (e) the concentration of M1 is 4 mM, (f) the concentration of M1 is 2 mM
[0038] Fig.14 The UV-visible absorption spectra of the present invention when Zn(OTf)2 is added dropwise to the solution of monomers A4, B4 and M1; (a) Zn(OTf)2 is added dropwise to the solution of A4+B4+M1 (CHCl3:DMSO=5:1, the concentration of M1 is 0.01mM); (b) Zn(OTf)2 is added dropwise to the mixed solution of B4+M1 (CHCl3:DMSO=5:1, the concentration of M1 is 0.01mM); (c) and (d) are relationship diagrams of the concentration of Zn(OTf)2 added dropwise to the solution and the UV absorption intensity of the solution;
[0039] Fig.15The present invention adds Zn(OTf)2 to A4+B4+M1 at an excitation wavelength of 294 nm, and measures the fluorescence emission intensity emission spectrum;
[0040] Fig.16 The A4+B4+M1 solution of the present invention is used to titrate Zn 2+ During the process, the CIE diagram of the solution fluorescence emission color change;
[0041] Fig.17 This is a photograph of the fluorescence change of the solution after adding Zn(OTf)2, TBAOH and TFA to the solution of A4+B4+M1 under 365nm ultraviolet light;
[0042] Fig.18 is a SEM photo of a representative sample prepared by freeze drying of the present invention;
[0043] Fig.19 It is a schematic diagram of the reversible transformation of the supramolecular polymer gel of the present invention. DETAILED DESCRIPTION
[0044] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0045] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0046] In the description of the present invention, it should be understood that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0047] like Figure 1-19As shown, a method for synthesizing supramolecular cross-linked polymers of pillared aromatics and terpyridine is provided, wherein the orthogonal non-covalent interaction between monomer M1, model compounds M2, M3 and Zn(OTf)2 in a mixed solvent of CDCl3 and DMSO-d6 is used to realize orthogonal self-assembly of monomers A4, B4, M1 and Zn(OTf)2 through complementary metal coordination interactions and host-guest reactions to form supramolecular cross-linked polymers of pillared aromatics and terpyridine.
[0048] A method for synthesizing a pillared aromatic hydrocarbon and terpyridine supramolecular cross-linked polymer comprises the following steps:
[0049] In an air atmosphere, 10 mmol A4, 10 mmol B4, 40 mmol M1 and 40 mmol Zn(OTf)2 were dissolved in a mixed solvent of CDCl3 and DMSO-d6, and the non-covalent interaction between A4, B4, M1 and Zn(OTf)2 was monitored by hydrogen nuclear magnetic resonance spectroscopy until the complexation was complete.
[0050] The synthetic route and chemical structure of the monomer are as follows:
[0051]
[0052] Synthesis of monomer A4:
[0053] Compound 2 (0.5 g, 0.48 mmol), compound 3 (1.55 g, 2.11 mmol), NaH (0.29 g, 7.20 mmol, sodium hydride, 60%) and KI (0.08 g, 0.48 mmol) were dissolved in 120 ml of DMF and stirred at 75 degrees Celsius for 12 hours under a nitrogen atmosphere. The reaction system was cooled and filtered, and the filtrate was collected and extracted with dichloromethane and water, dried over anhydrous sodium sulfate, and the solvent was removed by spin under reduced pressure. The crude product was purified with acetonitrile and dichloromethane (1 / 75, v / v) as eluents to obtain monomer A4 as a white solid.
[0054] 1 H NMR (400MHz, CDCl3) δ (ppm) = 6.96 (d, J = 8.7Hz, 8H), 6.84–6.78 (m, 40H), 6.65 (d, J = 8.8Hz, 8H), 3. 90–3.78(m,56H),3.71–3.65(m,108H),1.87–1.77(m,8H),1.75–1.66(m,8H),1.57–1.42(m,16H). 13C NMR (100MHz, CDCl3) δ157.42,150.66,150.03,136.93,132.65,128.37,114.92,113.89,68.47,67.71,55.91,29.61,26.25.MALDI-TOF-MS(C 226 H 252 O 44 ):m / z calcd for[M+H] + =3670.7482,found=3670.5100,error=6.5ppm.
[0055] Synthesis of monomer B4:
[0056] 1,2,4,5-benzene tetracarboxylic acid (0.1 g, 0.39 mmol) and 50 ml SOCl2 were added to a round-bottom flask, 0.3 ml DMF was added dropwise, and the mixture was stirred and refluxed at 80 degrees Celsius for 8 hours. The mixture was cooled and the solvent was removed by spin under reduced pressure to obtain an oily liquid, which was dissolved in 10 ml dry THF and slowly added dropwise to a round-bottom flask containing compound 5 (0.75 g, 1.60 mmol), 0.2 ml Et3N and 40 ml dry THF at 0 degrees Celsius. After the addition was complete, the mixture was stirred at 0 degrees Celsius for 12 hours, and then reacted at 25 degrees Celsius for 12 hours. The initial reaction product was extracted with dichloromethane and water, dried over anhydrous sodium sulfate, and the solvent was removed by spin under reduced pressure. The crude product was purified by column chromatography to obtain a white solid monomer B4.
[0057] 1 H NMR (400MHz, CDCl3) δ (ppm) = 8.85–8.60 (m, 24H), 8.08 (s, 2H), 7.94–7.82 (m, 16H), 7.41–7.31 (m,8H),7.06–6.97(m,8H),4.35(s,8H),4.01(s,8H),1.80(s,16H),1.43(d,J=45.2Hz,41H). 13 C NMR (100MHz, CDCl3) δ (ppm) = 166.11, 160.09, 156.35, 155.76, 149.71, 149.05, 136.82, 134.44, 130.39, 1 28.43,123.72,121.34,118.18,114.82,68.05,66.42,29.46,29.37,29.27,29.22,28.48,26.05,25.91.
[0058] MALDI-TOF-MS (C 130 H130 N 12 O 12 ):m / z calcd for[M] + =2052.5420,found=2052.8227,error=13.7ppm.
[0059] Synthesis of monomer M1:
[0060] Compound 8 (2.6 g, 3.84 mmol), 5-bromovaleronitrile (0.75 g, 4.61 mmol) and cesium carbonate (2.50 g, 7.68 mmol) were dissolved in 120 ml of DMF and stirred at 80 degrees Celsius for 12 hours under a nitrogen atmosphere. The reaction system was cooled and filtered, and the filtrate was collected and extracted with dichloromethane and water, dried over anhydrous sodium sulfate, and the solvent was removed by spin under reduced pressure. The crude product was purified by column chromatography to obtain a monomer CD as a yellow solid.
[0061] 1 H NMR (400MHz, CDCl3) δ (ppm) = 8.92 (d, J = 7.7Hz, 2H), 8.63 (s, 2H), 8.56 (s, 2H), 8.13 (t, J = 7.7Hz, 2H), 8.06 (d, J = 8.5Hz, 4H), 7.74 (d, J = 8.8Hz, 4H), 7 .54(dd,J=16.9,8.0Hz,4H),7.49–7.41(m,4H),7.41–7.31(m,4H),6.68(d ,J=8.8Hz,2H),3.80(t,J=5.5Hz,2H),2.30(t,J=6.8Hz,2H),1.77(m,4H).
[0062] Through the orthogonal non-covalent interaction between monomer M1, model compounds M2, M3 and Zn(OTf)2 in a mixed solvent of CDCl3 and DMSO-d6, monomers A4, B4, M1 and Zn(OTf)2 were orthogonally self-assembled to form pillar aromatic hydrocarbons and terpyridine supramolecular cross-linked polymers through complementary metal coordination interactions and host-guest reactions. M1, M2, and M3 were dissolved in a mixed solvent of CDCl3:DMSO-d6=5:1, and their nuclear magnetic resonance hydrogens were analyzed. M1 and M3 (molar ratio of 1:1) were dissolved in a mixed solvent of CDCl3:DMSO-d6=5:1, where the nuclear magnetic resonance signals of the H24, H25, and H26 protons on the alkyl chain of M1 all moved to the high field direction ( Fig. 9), proving that the neutral guest of the alkyl chain on M1 penetrated into the cavity of M3, and the host-guest interaction between M1 and M3 caused the two to complex. Then, M2, M1 and Zn(OTf)2 (molar ratio of 1:1:1) were dissolved in a mixed solvent of CDCl3:DMSO-d6=5:1, where the NMR signals of the H7 and H4 protons on M2 and the H19 and H15 protons on M1 all moved to the high field direction ( Fig.10 ), proving that the 9-anthryl-substituted terpyridine group (tey) on M1 and the terpyridine group (tpy) on M2 can undergo metal coordination in the presence of metal ions to form a stable complementary metal complex: tey-Zn 2+ -tpy. In addition, M1, M2, M3 and Zn(OTf)2 (molar ratio of 1:1:1:1) were dissolved in a mixed solvent of CDCl3:DMSO-d6=5:1, and the H NMR spectrum showed that ( Fig.11 ), two non-covalent interactions, namely the host-guest interaction between pillar[5]arene and neutral guests and the tey-Zn 2+ The complementary metal coordination effects of -tpy do not affect each other in the mixed solution and are orthogonal.
[0063] The chemical structure of monomer M1 is as follows:
[0064]
[0065] The chemical structure of the model compound M2 is as follows:
[0066]
[0067] The chemical structure of the model compound M3 is as follows:
[0068]
[0069] With the help of the H NMR spectrum of the model compound, A4+B4+M1+Zn 2+ The complex H NMR spectra can be accurately assigned.
[0070] A4, B4, M1 and Zn(OTf)2 were dissolved in a mixed solvent of CDCl3:DMSO-d6=5:1, and the H NMR spectrum was shown in the figure: Fig.12 The peak shapes of Hi, Hii, and Hiii protons on the aromatic hydrocarbons of the monomer M1 column [5] in a are compared with Fig.12b becomes broadened, and at the same time, the NMR signals of the H1, H2 and H3 protons on the alkyl chain of M1 all move toward the high field direction. The neutral guest on the alkyl chain of M1 penetrates into the cavity of M3. The host-guest interaction between M1 and M3 causes the two to complex. This phenomenon is consistent with the NMR hydrogen spectra of the model compounds M3 and M1. Figure 1 To;
[0071] On the other hand, the NMR signals of H7 and H8 protons on M1 all move toward the low field direction, and the NMR signals of He protons on B4 and H11 and H15 on M1 all move toward the high field direction, indicating that the monomers B4 and M1 form a stable complementary metal complex like the model compounds M1 and M2: tey-Zn 2+ In supramolecular polymer systems, the concentration of monomers has a crucial influence on the molecular weight and degree of polymerization of supramolecular polymers.
[0072] Based on the concentration-dependent H NMR spectrum of A4+B4+M1+Zn(OTf)2 ( Fig.13 ), with the increase of monomer concentration, the peak of H NMR spectrum gradually broadens, indicating that high molecular weight aggregates are gradually formed and constructed into supramolecular polymers.
[0073] The complementary metal coordination interactions in the supramolecular cross-linked polymer backbone can be further verified using UV-visible spectrophotometry. B4 and M1 were dissolved in a mixed solution of CHCl3 and DMSO (CHCl3:DMSO=5:1), with a molar ratio of B4 to M1 of 1:4, where the concentration of M1 was 0.015 mM. Zn(OTf)2 was then added dropwise to the solution, and the UV-visible absorption intensities of B4, M1, and Zn(OTf)2 were measured, as shown in Figure 3. Fig.14 The UV-visible absorption spectrum is plotted as shown in a. 2+ During the titration process, when the absorption wavelength is less than 312nm, as Zn 2+ With the increase of Zn concentration, its UV absorption intensity gradually decreases; when the absorption wavelength is greater than 312nm, the UV absorption intensity of the solution increases with the increase of Zn 2+ The concentration increases, and the two absorption peaks at 365nm and 384nm gradually disappear. 2+ When the concentration reaches 0.015 mM, the molar ratio of B4, M1 and Zn(OTf)2 is 1:4:4, the titration reaches the end point, the isosbestic point of the UV absorption peak appears at 310 nm, and the maximum absorption peak is at 347 nm; then continue to add Zn 2+ The absorption curve changes tend to be stable, indicating that the terpyridine group in monomer B4 and the 9-anthracenyl terpyridine group in monomer M1 are absorbed by Zn 2+The stoichiometric ratio of the three metals is 1:4:4. 2+ Add dropwise to the solution of A4, B4 and M1 (CHCl3:DMSO=5:1, v / v), and the obtained UV-visible absorption spectrum is ( Fig.14 b) Similar to the former, it shows the host-guest interaction between the pillar[5]arene in the A4 monomer and the neutral guest in the M1 monomer and the tey-Zn 2+ The complementary metal coordination effects of -tpy do not affect each other in the mixed solution and are orthogonal.
[0074] When the concentration of monomer M1 exceeds 60mM (A4:B4:M1:Zn(OTf)2=1:1:4:4), the supramolecular cross-linked polymer forms a supramolecular polymer gel. Due to the presence of non-covalent bonds, the supramolecular polymer gel will show responsiveness to external temperature stimulation, and the reversible conversion of sol-gel can be achieved by heating and cooling ( Fig.17 ). Because when heated, the supramolecular non-covalent bonds break, the supramolecular cross-linked network depolymerizes, and the spatial configuration of the supramolecular gel changes, which leads to the depolymerization of the gel to form a sol; after cooling, the non-covalent interactions are reformed, and the monomers re-self-assemble to form a supramolecular gel again, thus achieving a reversible transformation from gel to sol. Scanning electron microscopy (SEM) can observe the microscopic morphology of supramolecular cross-linked polymers. The structures of monomers A4 and B4 both contain long flexible methylene chains, and the molecules are easily entangled with each other to form interstitial cross-links to restrict molecular movement, so the supramolecular cross-linked polymer constructed by A4, B4, M1 and Zn(OTf)2 can form a gel at high concentrations. The prepared supramolecular cross-linked polymer is frozen using low-temperature liquid nitrogen, and then vacuumed on a freeze dryer to sublimate the solvent to prepare a dry gel sample. The freeze-dried sample was observed under a scanning electron microscope and found to have a three-dimensional network structure with many holes inside the gel. This is because the solvent originally fixed by the supramolecular polymer was sublimated under low temperature and low pressure conditions and left behind ( Fig.18 ).
[0075] The fluorescence properties of supramolecular cross-linked polymers can be tuned by various means. Fig.17 As shown, the solution of A4+B4+M1 emits strong blue fluorescence under 365nm ultraviolet light, which is attributed to the uncoordinated anthracene luminescent group on M1. Zn(OTf)2 was then added dropwise to the solution, and the fluorescence emission intensities of A4, B4, M1 and Zn(OTf)2 were measured, as shown in Figure 2. Fig.15 As shown in the figure, multiple fluorescence emission curves of A4, B4, M1 and Zn(OTf)2 at different Zn(OTf)2 concentrations were plotted. 2+With the increase of the content, the fluorescence emission intensity gradually decreased, and finally the solution color turned into light yellow and no longer emitted fluorescence. Fig.16 The CIE diagram of the solution luminescence color change during the titration process was plotted. This phenomenon is attributed to the terpyridine group in monomer B4 and the 9-anthryl terpyridine group in monomer M1 through Zn 2+ The complementary metal coordination structure is formed by the action of the hydroxyl group and the Zn 2+ Combined to form Zn(OH)2, so when TBAOH was subsequently added to the SCP solution, the solution again emitted strong blue fluorescence ( Fig.17 This phenomenon is due to the formation of zinc hydroxide, which destroys the tpy-Zn 2+ -tey structure, the coordinated tey is converted into free tey, and the anthracene group on the free tey group emits blue fluorescence under ultraviolet light. Adding trifluoroacetic acid (TFA) will make the fluorescence emission of the SCP solution disappear again. Then TFA is added to the above A4+B4+M1+Zn(OTf)2+TBAOH solution. TFA can react with Zn(OH)2 to generate zinc ions. The generation of zinc ions induces the metal coordination tpy-Zn 2+ The occurrence of -tey and the reconstruction of SCP lead to the quenching of fluorescence again ( Fig.17 ).
[0076] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0077] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for synthesizing a supramolecular cross-linked polymer of pillared aromatics and terpyridine, characterized in that: Through the orthogonal non-covalent interaction between monomer M1, model compounds M2, M3 and Zn(OTf)2 in a mixed solvent of CDCl3 and DMSO-d6, monomers A4, B4, M1 and Zn(OTf)2 were orthogonally self-assembled into pillar aromatics and terpyridine supramolecular cross-linked polymers through complementary metal coordination interactions and host-guest reactions. The chemical structure of M1 is as follows: The chemical structure of B4 is as follows; The chemical structure of A4 is as follows; The chemical structure of the model compound M2 is as follows: The chemical structure of the model compound M3 is as follows:
2. The method for synthesizing a supramolecular cross-linked polymer of pillared aromatics and terpyridine according to claim 1, characterized in that: The method comprises the following steps: dissolving 10 mmol A4, 10 mmol B4, 40 mmol M1 and 40 mmol Zn(OTf)2 in a mixed solvent of CDCl3 and DMSO-d6 in an air atmosphere, and monitoring the non-covalent interaction between A4, B4, M1 and Zn(OTf)2 by hydrogen nuclear magnetic resonance spectrum until the complexation is complete; The preparation method of monomer B4 comprises the following steps: 0.1 g of 1,2,4,5-benzenetetracarboxylic acid and 50 ml of SOCl2 were added to a round-bottom flask, 0.3 ml of DMF was added dropwise, and the mixture was stirred and refluxed at 80 degrees Celsius for 8 hours. The mixture was cooled and the solvent was removed by spin-drying under reduced pressure to obtain an oily liquid, which was dissolved in 10 ml of dry THF. The mixture was slowly added dropwise to a round-bottom flask containing 0.75 g of compound 5, 0.2 ml of Et3N and 40 ml of dry THF at 0 degrees Celsius. After the addition was completed, the mixture was stirred at 0 degrees Celsius for 12 hours, and then reacted at 25 degrees Celsius for 12 hours. The initial reaction product was extracted with dichloromethane and water, dried over anhydrous sodium sulfate, and the solvent was removed by spin-drying under reduced pressure. The crude product was purified by column chromatography to obtain monomer B4 as a white solid. The structure of compound 5 is as follows:
3. The method for synthesizing a supramolecular cross-linked polymer of pillared aromatics and terpyridine according to claim 2, characterized in that: The concentration of monomers has a crucial influence on the molecular weight and degree of polymerization of supramolecular polymers. Supramolecular cross-linked polymers with different molecular weights will be formed under different monomer concentrations. The higher the concentration, the larger the molecular weight of the supramolecular cross-linked polymer formed.
4. The method for synthesizing a supramolecular cross-linked polymer of pillared aromatics and terpyridine according to claim 2, characterized in that: The ratio of the CDCl3:DMSO-d6 mixed solvent is 5:
1.
5. The method for synthesizing a supramolecular cross-linked polymer of pillared aromatics and terpyridine according to claim 2, characterized in that: The terpyridine group in monomer B4 and the 9-anthryl terpyridine group in monomer M1 are reacted by Zn 2+ The effect of the two metals forms a stable complementary metal coordination structure.
6. The method for synthesizing a supramolecular cross-linked polymer of pillared aromatics and terpyridine according to claim 2, characterized in that: The 9-anthryl-substituted terpyridine group on the monomer M1 undergoes metal coordination with the terpyridine group on the model compound M2 to form a stable complementary metal complex tey-Zn 2+ -tpy; The monomers B4 and M1 and M1 and the model compound M2 form the same stable complementary metal complex tey-Zn 2 + -tpy.
7. The gel prepared by the method for synthesizing a supramolecular cross-linked polymer constructed of pillared aromatic hydrocarbons and terpyridine according to any one of claims 1 to 6, characterized in that: In an air atmosphere, A4, B4, M1, and Zn(OTf)2 were dissolved in a mixed solvent of CDCl3 and DMSO-d6 in a ratio of 1:1:4:
4. When the concentration of M1 exceeded 60 mM, the supramolecular cross-linked polymer formed a supramolecular polymer gel.