Packaging film and display panel
By using an encapsulation film with a porous structure of a solid oxygen film and a photocatalytic film on the OLED display panel, the problem of oxygen intrusion during the bending process of the flexible screen is solved, and effective protection and life extension of the OLED are achieved.
Patent Information
- Application Number
- CN202311136651.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-31
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-08-31
AI Technical Summary
Flexible and bendable screens are prone to cracks during multiple bending processes, which accelerates the aging of OLED organic light-emitting layer devices. They are also sensitive to water and oxygen, and require strict packaging to extend their lifespan and resist oxygen intrusion.
A solid oxygen film with a porous structure is used as the packaging film, including a metal organic complex and a photocatalytic film. The solid oxygen film absorbs oxygen through the pores, and the photocatalytic film decomposes water vapor to prevent oxygen from contacting the organic light-emitting unit.
Effectively absorb and fix external oxygen, reduce oxygen intrusion, extend the service life of OLED display panels, and improve stability and display quality.
Smart Images

Figure CN117062486B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of display technology, and in particular to a packaging film and a display panel. Background Art
[0002] Organic light emitting diode (OLED) has the advantages of surface light source, cold light, energy saving, fast response, flexibility, ultra-light and low cost, and its mass production technology is becoming increasingly mature. However, since OLED has poor stability and is extremely sensitive to water, oxygen and heat, packaging technology is particularly critical.
[0003] However, since flexible screens have to undergo multiple bending and deformation, cracks are prone to form in the encapsulation layer, which will accelerate the aging of OLED organic light-emitting layer devices. Therefore, strict encapsulation is necessary to extend the life and improve stability, and it is necessary to strictly resist oxygen intrusion to avoid failure of the organic light-emitting unit. Summary of the invention
[0004] In view of this, the present application provides a packaging film and a display panel, which can absorb the invading oxygen, so that the packaging film can play a good protective and packaging role.
[0005] In a first aspect, the present application provides a packaging film, the packaging film comprising:
[0006] First inorganic membrane;
[0007] an oxygen-solidifying membrane, the oxygen-solidifying membrane being disposed on one side of the first inorganic layer and being used for absorbing oxygen, the oxygen-solidifying membrane being a porous structure, the oxygen-solidifying membrane comprising holes, and the equivalent spherical diameter of the holes being in the range of 1 nm to 30 nm; and
[0008] The second inorganic film is stacked and arranged on a side of the solid oxygen film away from the first inorganic film.
[0009] Wherein, the solid oxygen film comprises a metal organic complex.
[0010] Wherein, the metal organic complex comprises one or more of a zirconium-based metal organic framework, an iron-based metal organic framework, a chromium-based metal organic framework, a zinc-based metal organic framework, and a magnesium-based metal organic framework;
[0011] The metal organic complex also includes a coordination metal and an organic ligand, wherein the coordination metal includes one or more of zirconium, iron, chromium, zinc, and magnesium, and the organic ligand includes one or more of biphenyl dicarboxylic acid, terephthalic acid, tetracarboxyphenyl porphyrin, tetrapyrene benzoate, and 2-methylimidazole.
[0012] Wherein, the solid oxygen membrane has a specific surface area S, and the specific surface area S satisfies: 500m 2 ·g -1 ≤S≤3000m 2 ·g -1 .
[0013] Wherein, along the stacking direction of the first inorganic film and the solid oxygen film, the solid oxygen film has a thickness range D1, and the thickness range D1 satisfies: 1 μm≤D1≤2 μm.
[0014] The oxygen-solidifying film comprises a plurality of filling parts and oxygen-solidifying parts, the plurality of filling parts are arranged at intervals from each other, the oxygen-solidifying parts are arranged around the periphery of each of the filling parts, and the light transmittance of the filling parts is greater than the light transmittance of the oxygen-solidifying parts.
[0015] Wherein, the encapsulation film further comprises a photocatalytic film, and the photocatalytic film is arranged between the oxygen-solidifying film and the second inorganic film, and is used for catalyzing the decomposition of water into hydrogen and oxygen.
[0016] The photocatalytic film comprises photocatalytic particles and a catalyst promoter material, the photocatalytic particles comprise graphite-phase carbon nitride, and the catalyst promoter material comprises supramolecular perylene tetracarboxylic acid.
[0017] Wherein, the photocatalytic film further comprises a plurality of nanofibers arranged in an interlaced manner, the photocatalytic particles are loaded on the nanofibers, and the auxiliary catalytic material is at least partially loaded on the photocatalytic particles.
[0018] In a second aspect, the present application further provides a display panel, the display panel comprising:
[0019] A light emitting unit, wherein the light emitting unit has a light emitting surface, and the light emitting surface is used for emitting light; and
[0020] The encapsulation film covers the light emitting surface of the light emitting unit and encapsulates and protects the light emitting unit.
[0021] The encapsulation film includes a first inorganic film, a solid oxygen film and a second inorganic film. When the encapsulation film is used to encapsulate and protect the organic light-emitting unit of the display panel, the first inorganic film can cover the organic light-emitting unit, and the solid oxygen film is arranged on the side of the first inorganic film adjacent to the display surface of the display panel, so that when the display panel has cracks from the display surface, the solid oxygen film can absorb and fix oxygen from the external environment to prevent oxygen from entering and contacting the organic light-emitting unit. And the solid oxygen film is a porous structure, the solid oxygen film includes holes, and the equivalent spherical diameter of the holes ranges from 1nm to 30nm, so that the solid oxygen film has good stability and a high specific surface area, so that the solid oxygen film can have abundant active sites to adsorb oxygen. When the encapsulation film has cracks, the solid oxygen film can efficiently absorb the invading oxygen and can absorb a large amount of oxygen, thereby reducing or avoiding the situation where oxygen invades the organic light-emitting unit, so that the encapsulation film can play a good protective and encapsulating role. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 is a schematic structural diagram of a display panel according to an embodiment of the present application;
[0024] Figure 2 is a schematic diagram of the cross-sectional structure of the encapsulation film according to an embodiment of the present application;
[0025] Figure 3 yes Figure 1 A schematic structural diagram of a cross section of a display panel along line AA provided in;
[0026] Figure 4 is a schematic structural diagram of a cross section of a display panel along line AA according to Embodiment 1 of the present application;
[0027] Figure 5 is a schematic structural diagram of a display panel in a cracked state according to an embodiment of the present application;
[0028] Figure 6 is a schematic diagram of the working principle of the display panel of the embodiment of the present application in a state where there are cracks;
[0029] Figure 7 is a schematic diagram of a partial structure of a photocatalytic film according to an embodiment of the present application;
[0030] Figure 8 is a schematic diagram of a portion of the structure of the nanofiber of an embodiment of the present application;
[0031] Fig. 9 is a schematic structural diagram of a cross section of a display panel along line AA according to Embodiment 2 of the present application;
[0032] Fig.10 It is a schematic diagram of the structure of the oxygen-solidifying membrane of an embodiment of the present application from a top view.
[0033] Description of reference numerals:
[0034] 1-display panel, 10-encapsulation film, 20-light-emitting unit, 30-display surface, 11-first inorganic film, 12-organic film, 13-oxygen-solidified film, 14-photocatalytic film, 15-second inorganic film, 21-light-emitting surface, 131-filling part, 132-oxygen-solidified part, 141-photocatalytic particles, 142-catalytic co-material, 143-nanofibers. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.
[0037] Reference to "embodiment" or "implementation" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiment or implementation may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0038] Before introducing the encapsulation film and the display panel provided by the embodiments of the present application, the related technologies are introduced.
[0039] In the related technology, OLED (Organic Light-Emitting Diode) device, that is, organic light-emitting diode, refers to an organic semiconductor device that emits light through carrier injection and recombination when organic semiconductor materials and luminescent materials are driven by an electric field. OLED has the characteristic of self-luminescence. The basic structure of OLED is to make a layer of organic luminescent material with a thickness of tens of nanometers on indium tin oxide (ITO) glass as a luminescent layer, and there is a metal electrode with a low work function above the luminescent layer.
[0040] The efficiency and life of OLED devices are closely related to the device structure. The structure widely used at present belongs to the "sandwich" structure, that is, the light-emitting layer is sandwiched between the cathode and the anode like a sandwich (one side is a transparent electrode to obtain a surface light-emitting effect). The first problem that needs to be solved to realize the commercialization of OLED is how to ensure the stable light emission of the device. Because the organic materials of OLED are very sensitive to substances such as water vapor and oxygen, various methods must be used to effectively encapsulate OLED devices to avoid contact between the device and water and oxygen, so as to reduce the aging rate of the device and extend the service life of the device.
[0041] See also Figures 1 to 6 , Figure 1 is a schematic diagram of the structure of a display panel according to an embodiment of the present application, Figure 2 is a schematic diagram of the cross-sectional structure of the encapsulation film of an embodiment of the present application, Figure 3 yes Figure 1 The schematic diagram of the structure of the cross section of the display panel along the AA line provided in FIG. Figure 4 is a schematic structural diagram of a cross section of a display panel along line AA according to Embodiment 1 of the present application, Figure 5 is a schematic structural diagram of a display panel in a cracked state according to an embodiment of the present application, Figure 6 The present application provides a packaging film 10, which includes a first inorganic film 11, an oxygen-fixing film 13, and a second inorganic film 15. The oxygen-fixing film 13 is disposed on one side of the first inorganic layer for absorbing oxygen. The oxygen-fixing film 13 is a porous structure, and the oxygen-fixing film 13 includes holes, and the equivalent spherical diameter of the holes ranges from 1 nm to 30 nm. The second inorganic film 15 is stacked on the side of the oxygen-fixing film 13 away from the first inorganic film 11.
[0042] The encapsulation film 10 may be, but is not limited to, used in an organic light-emitting diode (OLED) display panel 1, and is used to encapsulate and protect the organic light-emitting unit in the OLED display panel 1, so that the organic light-emitting unit is prevented from contacting oxygen and producing an oxidation reaction, which would otherwise damage the organic light-emitting unit. It is understandable that in other embodiments of the present application, the encapsulation film 10 may also be applied to other types of display panels 1, and the application scenario of the encapsulation film 10 should not be a limitation on the encapsulation film 10 provided in this embodiment.
[0043] Optionally, the encapsulation film 10 includes a first inorganic film 11, an oxygen-fixing film 13 and a second inorganic film 15. In one embodiment of the present application, the encapsulation film 10 may also include an organic film 12 and a photocatalytic film 14. Specifically, when the encapsulation film 10 is used to encapsulate and protect the light-emitting unit 20, the first inorganic film 11 may be arranged to cover the light-emitting unit 20, and the first inorganic film 11, the organic film 12, the oxygen-fixing film 13, the photocatalytic film 14 and the second inorganic film 15 are stacked in sequence. In other words, the organic film 12 is arranged on the surface of the first inorganic film 11 away from the light-emitting unit 20, the oxygen-fixing film 13 is arranged on the surface of the organic film 12 away from the first inorganic film 11, the photocatalytic film 14 is arranged on the surface of the oxygen-fixing film 13 away from the organic film 12, and the second inorganic film 15 is at least partially arranged on the surface of the photocatalytic film 14 away from the oxygen-fixing film 13.
[0044] Among them, the photocatalytic film 14 can decompose water vapor. Specifically, when the encapsulation film 10 does not produce cracks, the photocatalytic film 14 is in a closed environment and cannot perform a photocatalytic effect. When the display panel 1 is subjected to repeated bending and reaches its strength limit, irregular cracks will be generated in the encapsulation film 10. When the crack depth reaches the photocatalytic film 14, the photocatalytic particles 141 in the photocatalytic film 14 will undergo a photocatalytic decomposition of water to produce hydrogen on the surface of the photocatalytic particles 141 under the irradiation of visible light, that is, water vapor will be decomposed into hydrogen (H2) and oxygen (O2), and hydrogen (H2) and oxygen (O2) will be further discharged from the display panel 1 through the cracks, thereby avoiding further inward diffusion and extension of water vapor, which can effectively improve the service life of the display panel 1.
[0045] Optionally, the display panel 1 may have a display surface 30, and the solid oxygen film 13 is arranged on a side of the first inorganic film 11 adjacent to the display surface 30, so that when cracks are generated in the display panel 1 from the display surface 30, the solid oxygen film 13 can absorb and fix oxygen from the external environment to prevent oxygen from entering and contacting the organic light-emitting unit.
[0046] Optionally, the oxygen-fixing film 13 is also arranged on the side of the photocatalytic film 14 away from the display surface 30, so that after the photocatalytic film 14 decomposes water vapor into hydrogen and oxygen, the oxygen-fixing film 13 can also absorb and fix the oxygen generated by the photocatalytic film 14, thereby further preventing oxygen from entering and contacting the organic light-emitting unit.
[0047] Preferably, the material of the oxygen solid membrane 13 may be a material with a relatively high porosity, such as a metal organic framework (MOFs) material.
[0048] Among them, the metal organic framework compound (MOFs) material has many unique characteristics, such as ultra-low mass density, large pore volume and clear pore size distribution. Therefore, by changing the size of its component pores, the metal organic framework compound material can be used as an oxygen absorber, so that the solid oxygen film 13 can absorb oxygen efficiently and avoid oxygen contacting the organic light-emitting unit and causing it to fail.
[0049] Furthermore, the oxygen-solidifying membrane 13 is a porous structure, and the oxygen-solidifying membrane 13 may be but is not limited to having micropores and mesopores, so that the oxygen-solidifying membrane 13 has a higher specific surface area and abundant active sites.
[0050] Specifically, the oxygen solid film 13 includes holes, and the number of the holes can be multiple.
[0051] Optionally, the value of the equivalent spherical diameter of the hole can be but is not limited to 1nm, or 2nm, or 5nm, or 8nm, or 10nm, or 12nm, or 15nm, or 18nm, or 20nm, or 25nm, or 28nm, or 30nm, or other values, as long as the equivalent spherical diameter of the hole is in the range of 1nm to 30nm.
[0052] It can be understood that the equivalent spherical diameter is the diameter of an object having a shape and size similar to a sphere of the same volume. Optionally, the value of the equivalent spherical diameter can be understood as the average value of the equivalent spherical diameters of the multiple holes of the solid oxygen membrane 13.
[0053] When the equivalent spherical diameter of the hole is too small, the volume of the hole of the oxygen-fixing membrane 13 will be too small, which is not conducive to the absorption of a large amount of oxygen by the oxygen-fixing membrane 13, and the production cost of the oxygen-fixing membrane 13 will be high, which is not conducive to mass production. When the equivalent spherical diameter of the hole is too large, the specific surface area of the oxygen-fixing membrane 13 will be low, and the exposed active sites will be small, resulting in the overall activity of the oxygen-fixing membrane 13 being low, which is not conducive to oxygen adsorption, and thus the oxygen-fixing effect of the oxygen-fixing membrane 13 is not ideal.
[0054] In this embodiment, the equivalent spherical diameter of the hole ranges from 1 nm to 30 nm, so that the solid oxygen film 13 has good stability and a high specific surface area, so that the solid oxygen film 13 can have abundant active sites to adsorb oxygen. When the encapsulation film 10 has cracks, the solid oxygen film 13 can efficiently absorb the invading oxygen and can absorb a large amount of oxygen, thereby reducing or avoiding the situation where oxygen invades the organic light-emitting unit, so that the encapsulation film 10 can play a good protective role on the organic light-emitting unit.
[0055] In summary, in this embodiment, the encapsulation film 10 includes a first inorganic film 11, a solid oxygen film 13 and a second inorganic film 15. When the encapsulation film 10 is used to encapsulate and protect the organic light-emitting unit of the display panel 1, the first inorganic film 11 can cover the organic light-emitting unit, and the solid oxygen film 13 is arranged on the side of the first inorganic film 11 adjacent to the display surface 30 of the display panel 1, so that when the display panel 1 has cracks from the display surface 30, the solid oxygen film 13 can absorb and fix oxygen from the external environment to prevent oxygen from entering and contacting the organic light-emitting unit. And the solid oxygen film 13 is a porous structure, and the solid oxygen film 13 includes holes, and the equivalent spherical diameter of the holes ranges from 1nm to 30nm, so that the solid oxygen film 13 has good stability and a high specific surface area, so that the solid oxygen film 13 can have abundant active sites to adsorb oxygen. When cracks appear in the packaging film 10, the solid oxygen film 13 can efficiently absorb the invading oxygen and absorb a large amount of oxygen, thereby reducing or avoiding the invasion of oxygen into the organic light-emitting unit, so that the packaging film 10 can play a good protective and packaging role.
[0056] Optionally, the material of the first inorganic film 11 may include one or more of silicon oxide (SiO2), silicon oxynitride (SiOxNy) and silicon nitride (SiNx). It is understandable that the material of the first inorganic film 11 may also be composed of other materials, and the material composition of the first inorganic film 11 should not be a limitation on the encapsulation film 10 provided in this embodiment. Preferably, the first inorganic film 11 is a light-transmitting material.
[0057] Optionally, the material of the second inorganic film 15 may include silicon nitride (SiNx). It is understandable that the material of the second inorganic film 15 may also be composed of other materials, and the material composition of the second inorganic film 15 should not be a limitation on the encapsulation film 10 provided in this embodiment. Preferably, the second inorganic film 15 is a high-density silicon nitride (SiNx) film, which can have a good passivation effect, thereby effectively preventing the entry of external water vapor. Preferably, the second inorganic film 15 is a light-transmitting material.
[0058] It can be understood that when the display panel 1 is a flexible panel, the material of the second inorganic film 15 is easy to crack during bending due to its strong rigidity. The photocatalytic film 14 is arranged on the side of the second inorganic film 15 away from the display surface 30 of the display panel 1, and can effectively absorb the invading water vapor when cracks are generated in the display panel 1. The solid oxygen film 13 is arranged on the side of the photocatalytic film 14 away from the display surface 30, and can absorb the oxygen invading from the outside and the oxygen generated by the photocatalytic film 14 in the process of decomposing water vapor, thereby protecting the organic light-emitting unit from being corroded by oxygen and avoiding the failure of the organic light-emitting unit.
[0059] Optionally, the encapsulation film 10 may further include an organic film 12, which is sandwiched between the first inorganic film 11 and the solid oxygen film 13. The organic film 12 can not only inhibit the cracking of the first inorganic film 11 and the solid oxygen film 13, release the stress between inorganic substances, but also improve the flexibility and reliability of the entire encapsulation film 10. The solid oxygen film 13 is disposed on the side of the organic film 12 adjacent to the display surface 30, and can also protect the organic film 12 from corrosion by external oxygen.
[0060] Further optionally, the material of the organic film 12 may include one or more of acrylic (Polymethylmethacrylate, PMMA) or resin. It is understandable that the material of the organic film 12 may also be composed of other materials.
[0061] Please refer again Figure 4 The solid oxygen film 13 includes a metal organic complex.
[0062] Specifically, the metal organic complex may include a metal organic framework (MOFs) material.
[0063] In this embodiment, the metal organic complex is a metal organic framework compound (MOFs) material. The metal organic framework compound (MOFs) material has the characteristics of ultra-low mass density, large pore volume and clear pore size distribution. Therefore, by changing the size of its component pores, the metal organic framework compound (MOFs) material can be used as a good oxygen absorber to enable the solid oxygen film 13 to absorb oxygen efficiently and avoid the situation where oxygen contacts the organic light-emitting unit and causes its failure.
[0064] Please refer again Figure 4 The metal organic complex comprises one or more of a zirconium-based metal organic framework, an iron-based metal organic framework, a chromium-based metal organic framework, a zinc-based metal organic framework, and a magnesium-based metal organic framework;
[0065] The metal organic complex also includes a coordination metal and an organic ligand, wherein the coordination metal includes one or more of zirconium, iron, chromium, zinc, and magnesium, and the organic ligand includes one or more of biphenyl dicarboxylic acid, terephthalic acid, tetracarboxyphenyl porphyrin, tetrapyrene benzoate, and 2-methylimidazole.
[0066] Specifically, the metal organic complex may be, but is not limited to, one or more of a zirconium (Zr) based metal organic framework, an iron (Fe) based metal organic framework, a chromium (Cr) based metal organic framework, a zinc (Zn) based metal organic framework, and a magnesium (Mg) based metal organic framework.
[0067] The metal organic framework compound (MOFs) is a type of crystalline porous material with a periodic network structure formed by the interconnection of inorganic metal centers (metal ions or metal clusters) and bridging organic ligands through self-assembly.
[0068] Furthermore, the inorganic metal center, ie, the coordination metal, may be, but is not limited to, one or more of zirconium (Zr), iron (Fe), chromium (Cr), zinc (Zn), and magnesium (Mg).
[0069] Furthermore, the organic ligand may be, but is not limited to, one or more of biphenyl dicarboxylic acid (BPDC), terephthalic acid (BDC), tetracarboxyphenylporphyrin (M-TCPP), tetra-p-benzoylpyrene (TBAPy), and 2-methylimidazole (MelM).
[0070] Preferably, the metal organic complex is a metal organic framework compound (MOFs) material with high porosity and high specific surface area, such as UiO-67 material, UiO-66 material, PCN-600 (M) material, NU-1000 material, Cr-MIL-101 material, ZIF-8 material, Mg-MOF-74 material, or other materials.
[0071] The UiO-67 material may be composed of Zr6O4(OH)4 as a metal ligand and biphenyl dicarboxylic acid (BPDC) as an organic ligand.
[0072] The UiO-66 material may be composed of Zr6O4(OH)4 as a metal ligand and terephthalic acid (BDC) as an organic ligand.
[0073] The PCN-600(M) material may be composed of Fe3O(OH)3 as a metal ligand and tetracarboxyphenylporphyrin (M-TCPP) as an organic ligand.
[0074] The NU-1000 material may be composed of Zr6O4(OH)8(H2O)4 as a metal ligand and tetra(p-benzoyl)pyrene (TBAPy) as an organic ligand.
[0075] The Cr-MIL-101 material may be composed of Cr3O(OH)3 as a metal ligand and terephthalic acid (BDC) as an organic ligand.
[0076] The ZIF-8 material may be composed of Zn as a metal ligand and 2-methylimidazole (MelM) as an organic ligand.
[0077] The Mg-MOF-74 material may be composed of MgOH as a metal ligand and 2-hydroxyterephthalic acid (BDC-(OH)2) as an organic ligand.
[0078] In this embodiment, the metal organic complex includes a metal organic framework compound (MOFs), and the MOFs material can be, but is not limited to, one or more of UiO-67, UiO-66, PCN-600 (M), NU-1000, Cr-MIL-101, ZIF-8, or Mg-MOF-74. The solid oxygen film 13 composed of the above-mentioned MOFs material can effectively capture oxygen based on the porous structure advantage of the MOFs material, and is easy to apply to actual production, and the solid oxygen film 13 can have abundant active sites to adsorb oxygen. When cracks occur in the packaging film 10, the solid oxygen film 13 can efficiently absorb the invading oxygen and absorb a large amount of oxygen, so that the packaging film 10 can play a good protective and packaging role.
[0079] Optionally, the solid oxygen membrane 13 has a specific surface area S, and the specific surface area S satisfies: 500m 2 ·g -1 ≤S≤3000m 2·g -1 .
[0080] Optionally, the specific surface area S of the oxygen solid membrane 13 may be, but is not limited to, 500 m 2 ·g -1 , or 700m 2 ·g -1 , or 700m 2 ·g -1 , or 1000m 2 ·g -1 , or 1200m 2 ·g -1 , or 1500m 2 ·g -1 , or 1800m 2 ·g -1 , or 2000m 2 ·g -1 , or 2200m 2 ·g -1 , or 2500m 2 ·g -1 , or 2800m 2 ·g -1 , or 3000m 2 ·g -1 , or other values, as long as 500m 2 ·g -1 ≤S≤3000m 2 ·g -1 That's it.
[0081] When the specific surface area of the solid oxygen film 13 is small, the solid oxygen film 13 cannot expose enough active sites for oxygen adsorption, so that the solid oxygen film 13 absorbs less oxygen. When the packaging film 10 has cracks, the solid oxygen film 13 cannot fully absorb oxygen, which causes the components protected by the packaging film 10, such as the organic light-emitting unit, to still be at risk of being corroded by oxygen and failing. When the specific surface area of the solid oxygen film 13 is too large, the structural stability of the solid oxygen film 13 will be reduced, the toughness of the solid oxygen film 13 will be insufficient, and when the packaging film 10 is bent, the solid oxygen film 13 is prone to wrinkles or cracks, and the material components in the solid oxygen film 13 are prone to agglomeration, which makes the coating process prone to unevenness.
[0082] In this embodiment, the specific surface area S of the solid oxygen film 13 satisfies 500m 2 ·g -1 ≤S≤3000m 2 ·g -1, the solid oxygen film 13 can have good structural stability and expose sufficient active sites for oxygen adsorption, so that when cracks appear in the encapsulation film 10, the solid oxygen film 13 can fully and efficiently absorb oxygen, thereby avoiding the risk of the organic light-emitting unit being corroded by oxygen and failing, improving the reliability of the encapsulation film 10, and effectively ensuring the service life and excellent optical performance of the display panel 1.
[0083] Furthermore, the mass density of the solid oxygen film may be, but is not limited to, 0.13 g·cm -3 To 0.2 g·cm -3 , so that the solid oxygen membrane can have rich porosity and a lighter and thinner structural design.
[0084] Please refer again Figure 3 Along the stacking direction of the first inorganic film 11 and the solid oxygen film 13 , the solid oxygen film 13 has a thickness range D1 , and the thickness range D1 satisfies: 1 μm≤D1≤2 μm.
[0085] Optionally, the thickness range D1 may be understood as a maximum thickness value range of the oxygen-solidifying film 13 along a stacking direction of the first inorganic film 11 and the oxygen-solidifying film 13 .
[0086] Optionally, the thickness range D1 can be but is not limited to 1μm, or 1.1μm, or 1.2μm, or 1.3μm, or 1.4μm, or 1.5μm, or 1.6μm, or 1.7μm, or 1.8μm, or 1.9μm, or 2μm, or other values, as long as 1μm≤D1≤2μm is satisfied.
[0087] When the thickness of the oxygen-fixing film 13 is small, the oxygen-fixing film 13 cannot fully absorb the invading oxygen, and the structural stability of the oxygen-fixing film 13 is not strong, and it is easy to be damaged during the bending process. When the thickness of the oxygen-fixing film 13 is large, the overall thickness of the encapsulation film 10 will be large. When the encapsulation film 10 is applied to the display panel 1, it will be unfavorable for the display panel 1 to achieve the design requirements of being light and thin.
[0088] In this embodiment, the thickness range D1 of the solid oxygen film 13 satisfies 1μm≤D1≤2μm, so that the solid oxygen film 13 can meet the requirements of absorbing invading oxygen, thereby effectively protecting the performance of the organic light-emitting unit from being affected. The structure of the solid oxygen film 13 is relatively stable, so that the solid oxygen film 13 and the encapsulation film 10 have good bending resistance. And the thickness of the solid oxygen film 13 and the encapsulation film 10 will not be too high, which can meet the requirements of the thin and light design of the display panel 1, thereby improving the user experience.
[0089] See also Fig. 9 and Fig.10 , Fig. 9 is a schematic structural diagram of a cross section of a display panel along line AA according to Embodiment 2 of the present application, Fig.10 1 is a schematic diagram of the structure of the oxygen-fixing membrane of the embodiment of the present application from a top view. The oxygen-fixing membrane 13 includes a plurality of filling parts 131 and an oxygen-fixing part 132, wherein the plurality of filling parts 131 are arranged at intervals from each other, and the oxygen-fixing part 132 is arranged around the periphery of each of the filling parts 131, and the light transmittance of the filling part 131 is greater than the light transmittance of the oxygen-fixing part 132.
[0090] Optionally, the oxygen-solidifying portion 132 may be provided with the metal-organic complex material.
[0091] Preferably, the filling portion 131 may be provided with a transparent material, and the filling portion 131 may be made of a planarization layer material (PLN) commonly used in the display panel 1, such as a resin material, or polymethyl methacrylate (PMMA), or other materials.
[0092] Optionally, the number of the filling parts 131 may be but is not limited to two, three, four, five, six, or more. It is understandable that the number of the filling parts 131 should not be a limitation of the packaging film 10 provided in this embodiment.
[0093] It can be understood that the display panel 1 may include a plurality of organic light-emitting units arranged in an array, and the plurality of organic light-emitting units are arranged at intervals from each other. When the encapsulation film 10 is used to encapsulate and protect the organic light-emitting units of the display panel 1, since some metal organic complex materials themselves have colors, if the solid oxygen film 13 is directly opposite to the organic light-emitting unit, it may affect the display of the opening area of the display panel 1, that is, it will affect the normal light emission effect at the light emitting surface 21 of the organic light-emitting unit. Therefore, it is necessary to set the solid oxygen portion 132 outside the opening area of the display panel 1, that is, the solid oxygen portion 132 can be set in the gap between two adjacent organic light-emitting units.
[0094] It can be understood that in other embodiments of the present application, when the metal organic complex is selected from a material with high light transmittance, the oxygen-fixing portion 132 can be provided on the entire surface of the oxygen-fixing film 13 .
[0095] Further optionally, in one embodiment of the present application, the oxygen-fixing portion 132 may be an integral structure, the oxygen-fixing portion 132 may have a plurality of through holes, the filling portion 131 is filled in the through holes, and the oxygen-fixing portion 132 is arranged around the periphery of each of the filling portions 131 .
[0096] Further optionally, in another embodiment of the present application, the oxygen-solidifying membrane 13 may include a plurality of connected oxygen-solidifying portions 132 , the filling portion 131 may be disposed between two adjacent oxygen-solidifying portions 132 , and the oxygen-solidifying portion 132 is disposed around the periphery of each filling portion 131 .
[0097] In this embodiment, by setting the oxygen-fixing film 13 to a plurality of filling parts 131 and oxygen-fixing parts 132, when the encapsulation film 10 is applied to the display panel 1, the filling part 131 can be at least partially arranged opposite to the light-emitting surface 21 of the organic light-emitting unit, and the oxygen-fixing film 13 can be at least partially arranged opposite to the gap between two connected organic light-emitting units. And the light transmittance of the filling part 131 is greater than the light transmittance of the oxygen-fixing part 132, so that the oxygen-fixing film 13 can absorb the invading oxygen and effectively protect the performance of the organic light-emitting unit without affecting the normal light-emitting effect of the organic light-emitting unit, so as to improve the durability of the display panel 1 and ensure the excellent display quality of the display panel 1.
[0098] Please refer again Figure 4 , Figure 5 and Figure 6 The encapsulation film 10 further includes a photocatalytic film 14, which is disposed between the oxygen-solidifying film 13 and the second inorganic film 15, and is used for catalyzing the decomposition of water into hydrogen and oxygen.
[0099] Specifically, the photocatalytic film 14 includes photocatalytic particles 141 and a catalyst-assisting material 142. The photocatalytic particles 141 and the catalyst-assisting material 142 cooperate to catalyze water vapor for decomposition. Specifically, when the encapsulation film 10 does not produce cracks, the photocatalytic particles 141 are in a closed environment and cannot perform a photocatalytic effect. When the display panel 1 is subjected to repeated bending and reaches the strength limit, irregular cracks will be generated in the encapsulation film 10. When the crack depth penetrates the second inorganic film 15 of the top layer and reaches the photocatalytic film 14, the photocatalytic particles 141 and the co-catalytic material 142 will be exposed. When water vapor reaches the surface of the photocatalytic particles 141 and the co-catalytic material 142 through the cracks, a photocatalytic decomposition of water to produce hydrogen reaction will occur on the surface of the photocatalytic particles 141 under the irradiation of visible light, that is, water vapor will be decomposed into hydrogen (H2) and oxygen (O2), and hydrogen (H2) and oxygen (O2) will be further discharged from the display panel 1 through the cracks, thereby preventing the water vapor from further diffusing and extending inward.
[0100] In this embodiment, the photocatalytic film 14 is disposed between the oxygen-fixing film 13 and the second inorganic film 15. Optionally, the second inorganic film 15 can be disposed adjacent to the display surface 30 of the display panel 1. The photocatalytic film 14 is disposed on the side of the second inorganic film 15 away from the display surface 30, and is used to decompose the invading water vapor. The oxygen-fixing film 13 is disposed on the side of the photocatalytic film 14 away from the second inorganic film 15. The oxygen-fixing film 13 can not only absorb the oxygen invading from the outside, but also absorb and fix the oxygen generated by the photocatalytic film 14 after the photocatalytic film 14 decomposes the water vapor into hydrogen and oxygen, thereby further preventing oxygen from entering and contacting the organic light-emitting unit, thereby effectively extending the service life of the display panel 1 and ensuring the display quality of the display panel 1.
[0101] See also Figure 4 , Figure 7 and Figure 8 , Figure 7 is a partial structural schematic diagram of the photocatalytic film of the embodiment of the present application, Figure 8 The photocatalytic film 14 includes photocatalytic particles 141 and a catalyst-assisting material 142 . The photocatalytic particles 141 include graphite-phase carbon nitride, and the catalyst-assisting material 142 includes supramolecular perylene tetracarboxylic acid.
[0102] Optionally, the photocatalytic particles 141 can be composed of one or more of graphite phase carbon nitride particles (g-C3N4), boron nitride (BN), zinc oxide (ZnO) and titanium dioxide (TiO2). It can be understood that in other embodiments of the present application, the photocatalytic particles 141 can also be composed of other materials with good photocatalytic properties.
[0103] Preferably, the photocatalytic particles 141 are graphite phase carbon nitride particles (g-C3N4). Among them, the graphite phase carbon nitride particles (g-C3N4) have good thermal stability and chemical stability. The graphite phase carbon nitride particles (g-C3N4) can maintain stable performance at high temperatures, and the thermal stability will only begin to decrease when it exceeds 600°C. And the graphite phase carbon nitride particles (g-C3N4) can maintain stable performance under strong acids and bases. And as a new type of non-metallic photocatalytic particles 141, the graphite phase carbon nitride particles (g-C3N4) have a wider absorption spectrum range compared to traditional TiO2 photocatalysts, and do not require ultraviolet light, only under ordinary visible light can it play a photocatalytic role. Therefore, in this embodiment, graphite phase carbon nitride particles (g-C3N4) are selected as the photocatalytic particles 141, so that the packaging film 10 has excellent stability and durability, and is applicable to a wider range of scenarios. It also makes the photocatalytic film 14 have high catalytic efficiency, which can achieve rapid decomposition of water vapor, thereby ensuring the service life of the packaging film 10 protection element.
[0104] Optionally, the material of the co-catalytic material 142 can be composed of supramolecular perylenetetracarboxylic acid (PTA). Due to the high recombination rate of photogenerated electrons and holes in the graphite phase carbon nitride particles (g-C3N4), it is difficult to effectively improve the activity of the photocatalytic reaction. In this embodiment, by selecting supramolecular perylenetetracarboxylic acid (PTA) nanosheets as the co-catalytic material 142 of the graphite phase carbon nitride particles (g-C3N4), its photocatalytic hydrogen production activity can be significantly improved, so that the encapsulation film 10 can quickly decompose the invading water vapor, to further avoid the corrosion of the organic light-emitting layer caused by the invasion of water vapor into the organic light-emitting layer, thereby effectively extending the service life of the display panel 1, and allowing the display panel 1 to maintain excellent display quality.
[0105] Preferably, the photocatalytic film 14 has a light transmittance T, and the light transmittance T satisfies T≥70%, so that when the encapsulation film 10 is used for the display panel 1 , it will not affect the display quality of the display panel 1 .
[0106] Please refer again Figure 7 and Figure 8The photocatalytic film 14 further includes a plurality of nanofibers 143 arranged in a staggered manner, the photocatalytic particles 141 are supported on the nanofibers 143 , and the auxiliary catalytic material 142 is at least partially supported on the photocatalytic particles 141 .
[0107] Optionally, the material of the nanofiber 143 may be made of polyacrylonitrile (PAN), in other words, the nanofiber 143 may be polyacrylonitrile (PAN) nanofiber 143. It is understandable that in other embodiments of the present application, the material of the nanofiber 143 may also be other materials, such as polyvinyl pyrrolidone (PVP) or polyvinyl alcohol (PVA).
[0108] Further optionally, the nanofiber 143 can be prepared by using polyacrylonitrile (PAN) as a precursor liquid and an electrospinning process.
[0109] Optionally, the plurality of nanofibers 143 are staggered. Specifically, the plurality of nanofibers 143 may be prepared by an electrostatic spinning process and may be a material similar to a fiber membrane cloth.
[0110] Optionally, the photocatalytic film 14 may be made of the plurality of nanofibers 143 as a matrix material, and the plurality of nanofibers 143 may be staggered and overlapped to form a three-dimensional fiber film structure, so that the photocatalytic film 14 is an organic felt-like film with good ductility.
[0111] Optionally, the graphite phase carbon nitride particles are carried on the nanofibers 143, which can be understood as at least part of the graphite phase carbon nitride particles being attached to the surface of the nanofibers 143. The supramolecular perylene tetracarboxylic acid is carried on at least one of the nanofibers 143 or the graphite phase carbon nitride particles, which can be understood as part of the supramolecular perylene tetracarboxylic acid being attached to the surface of the nanofibers 143, and part of the supramolecular perylene tetracarboxylic acid being attached to the surface of the graphite phase carbon nitride particles. In other embodiments of the present application, the supramolecular perylene tetracarboxylic acid can also be entirely or mostly attached to the surface of the graphite phase carbon nitride particles, thereby effectively improving the photocatalytic efficiency of the graphite phase carbon nitride particles.
[0112] In this embodiment, the polyacrylonitrile (PAN) nanofibers 143 are used as carriers to load the graphite phase carbon nitride particles and the supramolecular perylene tetracarboxylic acid, so that the photocatalytic film 14 can be an organic felt-like film with good ductility, which can effectively increase the ductility of the encapsulation film 10, so that the encapsulation film 10 has a certain anti-bending effect, and the photocatalytic film 14 layer can be used as a toughness enhancement layer of the encapsulation film 10, further improving the durability of the encapsulation film 10 and the display panel 1.
[0113] Please refer again Figure 1 and Figure 4 A display panel 1, characterized in that the display panel 1 comprises a light emitting unit 20 and a packaging film 10, wherein the light emitting unit 20 has a light emitting surface 21, and the light emitting surface 21 is used to emit light. The packaging film 10 covers the light emitting surface 21 of the light emitting unit 20 and packages and protects the light emitting unit 20.
[0114] Optionally, the type of the display panel 1 may be an organic light-emitting diode (OLED) display panel. And the type of the OLED display panel 1 may be, but is not limited to, a passive matrix OLED display panel, an active matrix OLED display panel, a transparent OLED display panel, a top-emitting OLED display panel, a foldable OLED display panel, a white light OLED display panel, etc. It can be understood that in other embodiments of the present application, the display panel 1 may also be of other types, and the type of the display panel 1 should not be a limitation on the display panel 1 provided in this embodiment.
[0115] Optionally, the light-emitting unit 20 may be composed of an organic light-emitting material, such as a small molecule organic fluorescent substance, or a phosphorescent substance, or a polymer.
[0116] Optionally, the light emitting unit 20 has a light emitting surface 21 , and the light emitting surface 21 is used to emit light. The light emitting direction of the light emitting unit 20 may be but is not limited to the direction in which the light emitting unit 20 points to the packaging film 10 .
[0117] Further optionally, in one embodiment of the present application, the display panel 1 may be flexible and bendable. The encapsulation film 10 may cover the light emitting surface 21 of the light emitting unit 20, so as to encapsulate the light emitting unit 20, and during the bending process of the display panel 1, the light emitting unit 20 may be protected from being corroded by water vapor and oxygen.
[0118] Further optionally, in another embodiment of the present application, the display panel 1 may be a non-flexible package. The oxygen-fixing film 13 may be disposed at a position at the edge of the packaging film 10 where oxygen can easily enter.
[0119] In this embodiment, the encapsulation film 10 includes a first inorganic film 11, a solid oxygen film 13 and a second inorganic film 15. When the encapsulation film 10 is used to encapsulate and protect the organic light-emitting unit of the display panel 1, the first inorganic film 11 can cover the organic light-emitting unit, and the solid oxygen film 13 is arranged on the side of the first inorganic film 11 adjacent to the display surface 30 of the display panel 1, so that when the display panel 1 has cracks from the display surface 30, the solid oxygen film 13 can absorb and fix oxygen from the external environment to prevent oxygen from entering and contacting the organic light-emitting unit. The solid oxygen film 13 is a porous structure, and the solid oxygen film 13 includes holes, and the equivalent spherical diameter of the holes ranges from 1nm to 30nm, so that the solid oxygen film 13 has good stability and a high specific surface area, so that the solid oxygen film 13 can have abundant active sites to adsorb oxygen. When cracks appear on the encapsulation film 10, the solid oxygen film 13 can efficiently absorb the invading oxygen and absorb a large amount of oxygen, thereby reducing or avoiding the invasion of oxygen into the organic light-emitting unit, thereby reducing the damage of oxygen to the organic light-emitting unit, extending the service life of the display panel 1, and allowing the display panel 1 to maintain excellent display quality.
[0120] Mentioning "embodiment" and "implementation method" in this application means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrases in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments. In addition, it should also be understood that the features, structures or characteristics described in the various embodiments of the present application can be arbitrarily combined to form another embodiment that does not deviate from the spirit and scope of the technical solution of the present application, provided that there is no contradiction between them.
[0121] Finally, it should be noted that the above implementation modes are only used to illustrate the technical solution of the present application and are not intended to limit it. Although the present application has been described in detail with reference to the above preferred implementation modes, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present application.
Claims
1. A packaging film, characterized in that: The packaging film comprises: First inorganic membrane; An oxygen-solidifying membrane, which is disposed on one side of the first inorganic membrane and is used to absorb oxygen. The oxygen-solidifying membrane is a porous structure and includes pores. The equivalent spherical diameter of the pores ranges from 1 nm to 30 nm. a second inorganic film, the second inorganic film being stacked and disposed on a side of the oxygen solid film away from the first inorganic film; and A photocatalytic film, wherein the photocatalytic film is arranged between the solid oxygen film and the second inorganic film, and is used for catalyzing the decomposition of water into hydrogen and oxygen. The photocatalytic film comprises photocatalytic particles, a co-catalytic material and a plurality of nanofibers arranged in an alternating manner, wherein the material of the nanofibers comprises an organic material, the photocatalytic particles are loaded on the nanofibers, and the co-catalytic material is at least partially loaded on the photocatalytic particles.
2. The encapsulation film according to claim 1, characterized in that: The oxygen-solidifying film includes a metal-organic complex.
3. The encapsulation film according to claim 2, characterized in that: The metal organic complex is any one of a zirconium-based metal organic framework, an iron-based metal organic framework, a chromium-based metal organic framework, a zinc-based metal organic framework, and a magnesium-based metal organic framework; The metal organic complex also includes a coordination metal and an organic ligand, wherein the coordination metal includes one or more of zirconium, iron, chromium, zinc, and magnesium, and the organic ligand includes one or more of biphenyl dicarboxylic acid, terephthalic acid, tetracarboxyphenyl porphyrin, tetrapyrene benzoate, and 2-methylimidazole.
4. The encapsulation film according to claim 2, characterized in that: The solid oxygen membrane has a specific surface area S, and the specific surface area S satisfies: 500m 2 ·g -1 ≤S≤3000m 2 ·g -1 .
5. The encapsulation film according to claim 1, characterized in that: Along the stacking direction of the first inorganic film and the solid oxygen film, the solid oxygen film has a thickness range D1, and the thickness range D1 satisfies: 1 μm≤D1≤2 μm.
6. The encapsulation film according to claim 1, characterized in that: The oxygen-solidifying film includes a plurality of filling parts and an oxygen-solidifying part. The plurality of filling parts are arranged at intervals from each other. The oxygen-solidifying part is arranged around the periphery of each of the filling parts. The light transmittance of the filling part is greater than the light transmittance of the oxygen-solidifying part.
7. The encapsulation film according to claim 1, characterized in that: The photocatalytic particles include graphite-phase carbon nitride, and the co-catalytic material includes supramolecular perylene tetracarboxylic acid.
8. A display panel, characterized in that: The display panel comprises: A light emitting unit, wherein the light emitting unit has a light emitting surface, and the light emitting surface is used for emitting light; and The encapsulation film according to any one of claims 1 to 7, wherein the encapsulation film covers the light emitting surface of the light emitting unit and encapsulates and protects the light emitting unit.