An engineering preparation method and testing method for solution-aged Ti-6Al-6V-2Sn titanium alloy rod

Through forging and strict control of solid solution and aging processes, combined with Cu chips and V-Al-Fe ingredients, high-strength Ti-6Al-6V-2Sn titanium alloy rods are prepared, which solves the fatigue fracture and cooling of drill rods in complex wells. The precise problem achieves the high strength and hardenability of titanium alloy rods, meets petroleum drilling standards, and provides simple and accurate detection methods.

CN117070869BActive Publication Date: 2024-12-03CHONGQING SCI & INNOVATION CENT OF NORTHWEST POLYTECHNICAL UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311084377.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-28
Publication Date
2024-12-03
Estimated Expiration
2043-08-28

AI Technical Summary

Technical Problem

In complex structural wells, conventional drilling rods are fatigued and broken due to alternating stress, which cannot meet the operating needs of complex wells. Moreover, the cooling process of existing titanium alloy drilling rods is not accurate enough, which affects the detection of solid solution aging.

Method used

Adopt the forging process and strict control of solid solution and aging processes, including solid solution annealing and low temperature aging, to ensure the β-phase content ≥60%, and through rapid cooling and straightening processes, combining Cu chips and V-Al-Fe ingredients and smelting The number of times was used to prepare high-strength Ti-6Al-6V-2Sn titanium alloy rods, and detection methods were provided to evaluate hardness and mechanical properties.

Benefits of technology

The prepared titanium alloy rod has high strength, straightness and hardening properties, meets petroleum drilling standards, is simple and accurate in detection methods, is suitable for mass production, and significantly improves the strength and hardness of titanium alloy rods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117070869B_ABST
    Figure CN117070869B_ABST
Patent Text Reader

Abstract

The present invention discloses an engineering preparation method and testing method for a solution-aged Ti‑6Al‑6V‑2Sn titanium alloy bar, including forging and solution treatment of the solution-aged titanium alloy bar, the solution treatment temperature is Tβ‑(15~30)°C, and the holding time is 60min~120min; the bar after solution annealing is quickly cooled to obtain a fine structure, and the bar is taken out after it is completely cooled and the cooling time is ≥2h; the cooled bar is subjected to aging treatment. In order to produce solution-aged bars more simply, quickly, efficiently, and industrially, and to achieve the hardenability of the bars to a greater extent, the method proposed in the present invention controls the solution aging temperature, transfer time, and cooling water temperature through the heat treatment process, and simply and quickly detects the solution aging effect. It is suitable for the industrial production of titanium alloy bars of different specifications and diameters, and can also be used for the production and manufacturing of other solution-aged titanium alloy processing materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy processing, and in particular relates to an engineering preparation method and a testing method for a Ti-6Al-6V-2Sn titanium alloy bar in a solid solution-aging state. Background Art

[0002] In recent years, in order to improve the recovery rate of crude oil, reduce the cost of oil and gas field exploitation, and extend the development life of oil and gas fields, there are more and more complex wells, such as extended displacement wells, short radius horizontal wells, and horizontal wells with sidetracking of old wells. Conventional drill pipes have encountered some difficult problems when applied to these complex wells. For example, in ultra-short radius horizontal wells, the wellbore curvature is very small (<18 m), and conventional drill pipes produce large alternating stress. Fatigue fracture of drill pipes caused by alternating stress occurs from time to time, causing significant losses to oil fields. With the increasing number of ultra-deep wells, short radius wells and extended displacement wells, the service conditions of drill pipes in the wells are becoming more and more harsh, and conventional steel drill pipes can no longer meet the operational requirements of complex wells. In order to solve these problems, foreign countries have begun to start from new materials and develop titanium alloy drill pipes, aluminum alloy drill pipes, composite drill pipes, etc. to replace conventional drill pipes. Compared with traditional steel drill pipes, titanium alloy drill pipes have five advantages: lightweight, corrosion resistance, long life, high flexibility, and non-magnetic. The weight of titanium alloy drill pipe of the same specification is 57% of that of conventional steel drill pipe, which means that the drilling tools using titanium alloy drill pipe are lighter, and lower-level drilling rigs can be used for drilling construction, which can greatly save the daily fee of drilling rigs and thus reduce drilling costs.

[0003] Among titanium materials, industrial pure titanium (TA2 is the most widely used), Ti-6Al-4V (when a certain strength is required), and Ti-0.8Ni-0.3Mo (when there are gaps or in non-oxidizing media) are used in oil and gas drilling. In recent years, oil and gas drilling technology has developed rapidly. In order to further improve the drilling speed, ensure the drilling quality, and better adapt to the complex mining environment, high-strength drill pipe is one of the bottlenecks of oil drilling technology. The tensile strength of Ti-662 alloy is greater than 1000MPa, the yield strength is greater than 950MPa, the strength is higher than Ti-6Al-4V, the corrosion resistance is excellent, the welding and processing performance is medium, and it is used for aircraft fuselages, rocket engines, and nuclear reactor components. In recent years, the application growth rate in oil drilling has been significant. At the same time, the alloy has a certain heat resistance. In recent years, the demand for the use of this alloy in oil drilling has gradually increased at home and abroad. GE and Baker Hughes abroad have an urgent demand for such products.

[0004] GB / T225 "End quenching test method for steel hardenability (Jominy test)" introduces the method for determining the hardenability of steel. This method has high requirements for the test environment and the accuracy of each test process parameter. In order to better prepare solid solution aged bars in batches and engineering, the solid solution aging degree of the bars is quickly and accurately detected to ensure that the process is simple and clear, and the distribution of the test results is clear and intuitive. It is particularly important to invent a simple method that is universal for solid solution aged alloys through solid solution aging process control (control of primary α phase and secondary α phase content) and simple and efficient addition methods. Summary of the invention

[0005] In order to solve the technical problems existing in the above-mentioned background technology, the first aspect of the present invention provides an engineering preparation method of a Ti-6Al-6V-2Sn titanium alloy bar in a solid solution-aged state, comprising the following steps:

[0006] Step 1: bar preparation: the Ti-662 alloy ingot obtained by smelting is forged to obtain a Ti-662 alloy bar with uniform structure;

[0007] Step 2: Solution treatment: The Ti-662 alloy rod is subjected to solution annealing, the solution temperature is 15°C to 30°C below the β phase transformation point, the holding time is 60min to 120min, and the selection of the solution temperature and the holding time needs to ensure that the β phase content is controlled at a volume fraction of ≥60%; the rod is loaded after the furnace temperature is stabilized to the set temperature during the solution process, and the furnace door is closed and the heat treatment time is calculated after the furnace temperature is stabilized to the set temperature; the rod after solution treatment is quickly transferred to cooling water for cooling, the cooling water level needs to completely submerge the rod, stir quickly after entering the water, and continue to inject water to ensure that the water temperature is ≤40°C, and the rod is taken out after entering the water for ≥2h and completely cooled;

[0008] Step 3: Aging treatment: The bar that has been completely cooled in step 2 is subjected to low-temperature aging.

[0009] Furthermore, when the raw materials are smelted in step 1, Cu chips and the intermediate alloy V-Al-Fe are used to prepare, mix and feed the raw materials twice, and finally the raw materials are pressed. The smelting times are 2 to 3 times.

[0010] Furthermore, the forging process in step 1 specifically includes: heating the Ti-662 alloy ingot obtained by smelting in a natural gas furnace in stages and keeping it warm for a period of time before taking it out of the furnace, performing blank forging and multi-fire upsetting forging at 100-200°C above the phase transformation point, and then performing multi-fire forging at 30-60°C below the phase transformation point; the forging rate of the entire forging process is 20-30 mm / s, and the final forging temperature is ≥800°C.

[0011] Furthermore, in step 1, the holding time used for heating the forging billet above the phase transformation point is the billet cross-sectional size × 0.5~0.6min, and the holding time used for heating the forging billet below the phase transformation point is the billet cross-sectional size × 0.7~0.8min.

[0012] Furthermore, the holding time of the solution treatment in step 2 is the cross-sectional size of the rod × 1.5 min.

[0013] Furthermore, in step 2, the transfer time used for quickly transferring the rod to the cooling water is less than 40s, and the cooling rate is greater than 50°C / s.

[0014] Furthermore, in step 3, the aging treatment temperature range is 510°C to 600°C, the insulation time is 4h to 8h, and air cooling is performed after the insulation is completed.

[0015] Furthermore, the method further comprises: adding a straightening process after the solution treatment in step 2, the straightening temperature is 700° C. to 750° C., the insulation time is 30 min to 1 h, and the residual heat is used for straightening after the insulation is completed.

[0016] A second aspect of the present invention provides a method for testing a solution-aged Ti-6Al-6V-2Sn titanium alloy bar, comprising:

[0017] A sample piece is cut from the cross section of the rod prepared by the above method, and a suitable hardness test method is selected to perform hardness tests along the outer circle of the rod toward the center of the circle, and the change pattern of the hardness data is observed; at the same time, a tensile specimen is taken from the center of the rod for room temperature mechanical property testing and microstructure observation.

[0018] Furthermore, during the test sampling process, the end-affected areas at both ends of the rod need to be removed, and the removal amount is greater than the rod diameter.

[0019] Compared with the prior art, the present invention has the following beneficial technical effects:

[0020] 1. The present invention can produce corresponding specifications of solution-aged bars through forging process, solution and aging process control, and the β-phase content of the bars is ≥60%, and the grain size rating is ≥8 (judged according to ASTM E112). At the same time, after strict solution aging process control, the straightness of the prepared bars is ≤1mm / m, which fully meets the requirements of oil drilling and logging standards.

[0021] 2. The method for determining the hardenability of steel is introduced in GB / T225 "End Quenching Test Method for Hardenability of Steel (Jominy Test)". This method has high requirements for the test environment and the accuracy of the test process parameters. At the same time, due to the small cross-sectional size of the sample, the accuracy of each link has a greater impact on the final result. The preparation and testing method of the present invention can quickly and accurately detect the degree of solid solution aging of the bar, the hardness data detection process is simple and clear, and the distribution of the test results is clear and intuitive.

[0022] 3. This invention is generally applicable to batch and engineering preparation of solution-aged bars. The invention content clarifies the forging points of Ti-662 alloy bars, and gives recommended solution and aging treatment temperatures, holding times, cooling parameters, result detection methods and other process details, which can ensure the strength and hardness of solution-aged bar products, and can also further promote this simple testing method. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the microstructure diagram of the Ti-662 alloy Φ50×3000mm bar in Example 1 of the present invention.

[0024] Figure 2 This is the hardness test curve of the Ti-662 alloy Φ50×3000mm bar in Example 1 of the present invention.

[0025] Figure 3 This is the microstructure diagram of the Ti-662 alloy Φ90×3000mm bar in Example 2 of the present invention.

[0026] Figure 4 This is the hardness test curve of the Ti-662 alloy Φ90×3000mm bar in Example 2 of the present invention.

[0027] Figure 5 Schematic diagram of hardness sampling of Ti-662 alloy rod in an embodiment of the present invention. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In order to produce solution-aged bars more simply, quickly, efficiently and industrially and achieve the hardenability of the bars to a greater extent, the present invention proposes a method for controlling the solution-aging temperature, transfer time and cooling water temperature through a heat treatment process, which can simply and quickly detect the solution-aging effect. The method is suitable for the industrial production of titanium alloy bars of different specifications and diameters, and can also be used for the production of other solution-aged titanium alloy processed materials.

[0030] The first aspect of the present invention provides an engineering preparation method for a solution-aged Ti-6Al-6V-2Sn titanium alloy bar, comprising the following steps:

[0031] Step 1: bar preparation: the Ti-662 alloy ingot obtained by smelting is forged to obtain a Ti-662 alloy bar with uniform structure;

[0032] Step 2: Solution treatment: Solution annealing is performed on the Ti-662 alloy rods. The solution temperature is 15℃~30℃ below the β phase transformation point. The holding time is 60min~120min. The selection of the solution temperature and the holding time must ensure that the β phase content is controlled at a volume fraction of ≥60%; the rods are loaded after the furnace temperature is stabilized to the set temperature during the solution process. The furnace door is closed and the heat treatment time is calculated after the furnace temperature stabilizes to the set temperature; the rods after solution treatment are quickly transferred to cooling water for cooling. The cooling water level must completely submerge the rods. After entering the water, stir quickly and continue to inject water to ensure that the water temperature is ≤40℃. The rods are taken out after entering the water for ≥2h and completely cooled;

[0033] Step 3: Aging treatment: The bar that has been completely cooled in step 2 is subjected to low-temperature aging.

[0034] The above-mentioned solid solution temperature can be, for example, 15°C, 18°C, 22°C, 25°C, 30°C, etc. below the β phase transformation point; the insulation time can be, for example, 60min, 75min, 90min, 105min, 120min, etc.

[0035] In some embodiments, the temperature of the water entering the cooling water in step 2 when the rod is quickly transferred to the cooling water may be 18°C-22°C, for example, 18°C, 19°C, 20°C, 22°C, etc. The transfer time used is less than 40s, and may be 30-38s, for example, 30s, 36s, 38s, etc. The cooling rate is greater than 50°C / s, and may be 75-90°C / s, for example, 75°C / s, 80°C / s, 85°C / s, 90°C / s, etc.

[0036] In the solid solution treatment stage of titanium alloy bars in the existing ordinary engineering or laboratory stage, the water temperature and water conditions for cooling are not set accurately enough, resulting in large fluctuations in the water entry stage. The temperature difference after entering the water is different, which makes the internal stress of the bar very large, resulting in bending and deformation problems in the bars after solid solution treatment. In addition, if the water temperature and speed of entering the water are not well controlled, it will also have a great impact on the degree of solid solution aging. Based on this, the cooling stage during the solid solution treatment proposed by the present invention can fully solve the bending and deformation problems of the bars after solid solution treatment by strictly controlling the water temperature, water conditions and cooling rate of the water, etc., and is particularly suitable for large-sized titanium alloy bars of Ф25mm-Ф120mm×2000mm-3000mm.

[0037] In some embodiments, when low-temperature aging is performed, the aging temperature is selected according to the strength and other indicators required by the rod. The general principle is that the aging temperature is not lower than the service condition temperature, and the aging time must ensure that the aging precipitation has enough time to complete to achieve the aging effect. Specifically, the aging treatment temperature range in step 3 is 510℃~600℃, for example, it can be 510℃, 520℃, 550℃, 580℃, 600℃, etc.; the insulation time is 4h~8h, for example, it can be 4h, 5h, 6h, 7h, 8h, etc.; after the insulation is completed, it is dispersed and air-cooled.

[0038] In some embodiments, when the raw materials are smelted in step 1, according to the segregation characteristics of Cu and Fe elements, Cu chips and the intermediate alloy V-Al-Fe are used to prepare, mix and feed the materials twice, and finally the materials are pressed, and the smelting times are 2 to 3 times.

[0039] In some embodiments, the forging process in step 1 specifically includes: heating the Ti-662 alloy ingot obtained by smelting in a natural gas furnace in stages and keeping it warm for 180 minutes before taking it out of the furnace, performing open forging and multi-fire upsetting forging at 100~200°C above the phase transformation point, and then performing multi-fire forging at 30~60°C below the phase transformation point; the forging rate of the entire forging process is 20~30mm / s, and the final forging temperature is ≥800°C.

[0040] The above-mentioned blank forging temperature can be, for example, 100°C, 130°C, 150°C, 180°C, 200°C, etc. above the phase transformation point; the temperature of multi-fire forging can be, for example, 30°C, 40°C, 50°C, 60°C, etc. below the phase transformation point; the forging rate of the entire forging process can be, for example, 20mm / s, 23mm / s, 26mm / s, 30mm / s, etc.

[0041] The entire forging process of the present invention controls the billet heating time, holding time, deformation amount, forging rate and final forging temperature. At the same time, through the high-low-high deformation and heat treatment process, the uniformity of the structure and deformation consistency of the free forging billet are guaranteed, the structure of the intermediate billet is refined, the influence range of the difficult deformation zone is reduced, and the necessary basis is provided for the subsequent heat treatment of the bar.

[0042] In some embodiments, the holding time used for heating the forging billet above the phase transformation point in step 1 is the billet cross-sectional size × 0.5~0.6min, and the holding time used for heating the forging billet below the phase transformation point is the billet cross-sectional size × 0.7~0.8min.

[0043] In some embodiments, the holding time of the solution treatment in step 2 is the cross-sectional size of the rod × 1.5 min.

[0044] In some embodiments, considering that the residual stress of the rod after entering the water during the solution treatment process is relatively large, according to the actual situation of the rod, the above preparation method may also include: adding a straightening process after the solution treatment in step 2, the straightening temperature is 700°C~750°C, the insulation time is 30min~1h, and the residual heat is used for straightening after the insulation is completed.

[0045] A second aspect of the present invention provides a method for testing a solution-aged Ti-6Al-6V-2Sn titanium alloy bar, comprising:

[0046] A sample piece is cut from the cross section of the rod prepared by the above method, and a suitable hardness test method is selected to perform hardness tests along the outer circle of the rod toward the center of the circle, and the change pattern of the hardness data is observed; at the same time, a tensile specimen is taken from the center of the rod for room temperature mechanical property testing and microstructure observation.

[0047] In some embodiments, during the test sampling process, the end impact areas at both ends of the rod need to be removed, and the removal amount is greater than the rod diameter. At the same time, the hardness test should be recorded after removing the contamination layer on the surface of the rod. Specifically, after the rod is treated with solid solution aging and the surface contamination layer is removed, the micro-Vickers hardness is tested, specifically, three data are tested every 120° position and every 1.5mm along the outer circle of the rod to the center, and the average value is taken as the final hardness test data of the rod.

[0048] GB / T225 "End Quenching Test Method for Hardenability of Steel (Jominy Test)" introduces the method for determining the hardenability of steel. This method has high requirements for the test environment and the accuracy of the parameters in each test process. At the same time, due to the small cross-sectional size of the specimen, the accuracy of each link has a greater impact on the final result. The test method provided above can quickly and accurately detect the degree of solid solution aging of the bar. The hardness data detection process is simple and clear, and the distribution of the test results is clear and intuitive.

[0049] The following is explained in conjunction with specific embodiments:

[0050] The two groups of embodiments provided by the present invention respectively use rods of different specifications of Ti-662 alloy. The two specifications of the rods are respectively subjected to solution treatment, aging treatment and hardness test, and the microstructure and properties after ordinary heat treatment are compared, ultimately achieving a substantial improvement in indicators such as strength and hardness.

[0051] Embodiment 1

[0052] The implementation object of this embodiment is Ti-662 alloy Ф50mm specification bar, and the specific process is as follows:

[0053] Step 1: Bar preparation. After high temperature homogenization treatment of the ingot, it is forged on a 3150t free forging machine and finished on a SXP-13 horizontal precision forging machine. β The temperature of the finished product is 950℃ and the forging temperature of the finished product is 910℃. The bars are formed by drawing and beating, with a forging speed of 3.2m / min. The bars are forged to a size of Ф50×3300mm and then air-cooled on a rack.

[0054] Step 2: Solution treatment. The Ti-662 alloy bar with a size of 50×3300mm was solution treated in a resistance heating furnace with an accuracy of ±5℃. The heat treatment temperature was 920℃ and the temperature was kept for 60min to ensure that the primary α (α p ) content is controlled at ≤30% (the technical indicator requires that the β phase content is not less than 60%, volume fraction). The furnace is loaded at temperature, and the timing starts when the furnace temperature stabilizes to 920℃ after loading. After the insulation is completed, the furnace door is opened and the rods are immediately transferred to the water tank for cooling. The transfer time is 38s. The water temperature is 19℃ when entering the water, and the cooling rate is about 90℃ / s. After 2h of insulation, the rods are completely cooled and fished out, and the outlet water temperature is 21℃.

[0055] Step 3: Aging treatment. The Ti-662 alloy bars with a size of Ф50×3300mm are aged in a resistance heating furnace with an accuracy of ±3℃. The aging temperature is 580℃ and the insulation time is 8h. The furnace is loaded at the temperature, and the timing starts when the furnace temperature stabilizes to 580℃ after loading. After the insulation is completed, the bars are taken out of the furnace and placed on the rack for air cooling.

[0056] Step 4: Hardness test. After cutting off the shrinkage tail and the affected area at one end of the bar (overall removal> 50mm), cut a 15mm thick hardness test specimen, machine the cross section to a roughness of Ra≤3.2um, remove the contamination layer on the outer surface (about 2mm thick), and then perform microhardness tests at intervals of 1.5mm every 120°.

[0057] Evaluation of solution aging results: Microhardness, room temperature mechanical properties and microstructure observation were performed on Ti-662 alloy bars with a diameter of 50×3300mm. The microhardness test method refers to the standard ASTM E384 (test method for microindentation hardness of materials), and the room temperature mechanical properties test method refers to the standard ASTM E8 / E8M (tensile test method for metal materials). Microstructure observation refers to the standards AMS2380 and ASTM E112. The test data after solution aging treatment and ordinary annealing are shown in Table 1. It can be clearly seen from the data in Table 1 that after solution aging treatment, the strength of the bars is generally increased by more than 250MPa, the Vickers hardness is increased from 333 to more than 400, and the plasticity index does not change much.

[0058] Table 1 Comparison of Ti-662 alloy Ф50mm bar in different states

[0059]

[0060] Embodiment 2

[0061] The object of this embodiment is Ti-662 alloy 90mm diameter bar, and the specific process is as follows:

[0062] Step 1: Bar preparation. After high temperature homogenization treatment of the ingot, it is forged on a 3150t free forging machine and finished on a SXP-13 horizontal precision forging machine. β The temperature of the finished product is 950℃ and the forging temperature of the finished product is 910℃. The bar is formed by drawing and beating, and the forging speed is 3.2m / min. The bar size is forged to Ф90×3300mm and then air-cooled on the rack.

[0063] Step 2: Solution treatment. The Ti-662 alloy bar with a size of 90×3300mm was solution treated in a resistance heating furnace with an accuracy of ±5°C. The heat treatment temperature was 920°C and the temperature was kept for 120 minutes to ensure that the primary α (α p ) content is controlled at ≤30% (the technical indicator requires that the β phase content is not less than 60%, volume fraction). The furnace is loaded at temperature, and the timing starts when the furnace temperature stabilizes to 920℃ after loading. After the insulation is completed, the furnace door is opened and the rods are immediately transferred to the water tank for cooling. The water temperature is 20℃ when entering the water, the transfer time is 36s, and the cooling rate is about 75℃ / s. After 2h of insulation, the rods are completely cooled and fished out, and the outlet water temperature is 23℃.

[0064] Step 3: Aging treatment. The Ti-662 alloy bars with a size of 90×3300mm are aged in a resistance heating furnace with an accuracy of ±3℃. The aging temperature is 520℃ and the holding time is 8h. The furnace is loaded at the temperature, and the timing starts when the furnace temperature stabilizes to 520℃ after loading. After the insulation is completed, the bars are taken out of the furnace and placed on the rack for air cooling.

[0065] Step 4: Hardness test. After cutting off the shrinkage tail and the affected area at one end of the bar (overall removal> 100mm), cut a 15mm thick hardness test specimen, machine the cross section to a roughness of Ra≤3.2um, remove the contamination layer on the outer surface (about 2mm thick), and perform microhardness tests at intervals of 120° and 1.5mm.

[0066] Evaluation of solution aging results: Microhardness, room temperature mechanical properties and microstructure observation were performed on Ti-662 alloy bars with a diameter of 90×3300mm. The microhardness test method refers to the standard ASTM E384 (test method for microindentation hardness of materials), and the room temperature mechanical properties test method refers to the standard ASTM E8 / E8M (tensile test method for metal materials). Microstructure observation refers to the standards AMS2380 and ASTM E112. The test data after solution aging treatment and ordinary annealing are shown in Table 2. It can be clearly seen from the data in Table 2 that after solution aging treatment, the strength of the bars generally increased by more than 150MPa, the Vickers hardness increased from 328 to 395, and the plasticity index did not change much.

[0067] Table 2 Comparison of Ti-662 alloy 90mm bar in different states

[0068]

[0069] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An engineering preparation method for a solution-aged Ti-6Al-6V-2Sn titanium alloy bar, characterized in that: The steps include: Step 1: bar preparation: forging the Ti-6Al-6V-2Sn alloy ingot obtained by smelting to obtain a Ti-6Al-6V-2Sn alloy bar with uniform structure; Step 2: Solution treatment: The Ti-6Al-6V-2Sn alloy rod is subjected to solution annealing, the solution temperature is 15°C to 30°C below the β phase transformation point, the holding time is 60min to 120min, and the selection of the solution temperature and the holding time needs to ensure that the β phase content is controlled at a volume fraction of ≥60%; during the solution process, the rod is loaded after the furnace temperature is stabilized to the set temperature, and the furnace door is closed and the heat treatment time is calculated after the furnace temperature is stabilized to the set temperature; the rod after solution treatment is quickly transferred to cooling water for cooling, the transfer time used for the rod to be quickly transferred to the cooling water is <40s, the cooling rate is >50°C / s, the water temperature of the rod to be quickly transferred to the cooling water is 18-22°C, the cooling water level needs to completely submerge the rod, stir quickly after entering the water, and continuously inject water to ensure that the water temperature is ≤40°C, and the rod is taken out after entering the water for ≥2h and completely cooled; After solution treatment, a straightening process is added, the straightening temperature is 700℃~750℃, the holding time is 30min~1h, and the residual heat is used for straightening after the holding is completed; Step 3: Aging treatment: subject the fully cooled bar in step 2 to low temperature aging; The testing method of the above-mentioned solution-aged Ti-6Al-6V-2Sn titanium alloy rod comprises: cutting a sample from the cross section of the prepared rod, selecting a suitable hardness testing method, performing hardness tests in sequence along the outer circle of the rod toward the center of the circle, and observing the change pattern of the hardness data; at the same time, taking a tensile specimen from the center of the rod for room temperature mechanical property testing and microstructure observation.

2. The engineering preparation method of the solution-aged Ti-6Al-6V-2Sn titanium alloy bar according to claim 1 is characterized in that: When the raw materials are smelted in step 1, Cu chips and the intermediate alloy V-Al-Fe are used to carry out batching, mixing and feeding in two times, and finally pressing is carried out, and the smelting times are 2 to 3 times.

3. The engineering preparation method of the solution-aged Ti-6Al-6V-2Sn titanium alloy bar according to claim 1 is characterized in that: The forging process in step 1 specifically includes: heating the Ti-6Al-6V-2Sn alloy ingot obtained by smelting in a natural gas furnace in stages and keeping it warm for a period of time before taking it out of the furnace, performing blank forging and multi-fire upsetting forging at 100-200°C above the phase transformation point, and then performing multi-fire forging at 30-60°C below the phase transformation point; the forging rate of the entire forging process is 20-30 mm / s, and the final forging temperature is ≥800°C.

4. The engineering preparation method of the solution-aged Ti-6Al-6V-2Sn titanium alloy bar according to claim 3 is characterized in that: In step 1, the holding time used for heating the forging billet above the phase transformation point is the billet cross-sectional size × 0.5~0.6min, and the holding time used for heating the forging billet below the phase transformation point is the billet cross-sectional size × 0.7~0.8min, and the unit of the billet cross-sectional size is mm.

5. The engineering preparation method of the solution-aged Ti-6Al-6V-2Sn titanium alloy bar according to claim 1 is characterized in that: In step 3, the aging treatment temperature range is 510°C~600°C, the insulation time is 4h~8h, and air cooling is performed after the insulation is completed.

6. The engineering preparation method of the solution-aged Ti-6Al-6V-2Sn titanium alloy bar according to claim 1, characterized in that: During the test sampling process, the end impact areas at both ends of the rod need to be removed, and the removal amount is greater than the rod diameter.

Citation Information

Patent Citations

  • Process for preparing Ti662 titanium alloy tube material

    CN104498849A

  • Method for freely forging Ti55531 titanium alloy large-specification bar material

    CN109454188A

  • Preparation method of TC6 titanium alloy large-sized bar

    CN113172115A

  • Forging method capable of improving fracture toughness of TB6 titanium alloy

    CN114042847A

  • Preparation method of nickel-based wrought superalloy wheel disk forgings used at high temperature

    US20220119931A1