A heterojunction interface electric field enhanced up-conversion luminescent material and preparation method thereof
By designing a highly lattice-matched BiOCl/BiOBr:Yb3+, Er3+ heterojunction structure in rare earth upconversion nanoparticles, and utilizing the internal electric field characteristics of bismuth oxyhalide, the problem of low luminous efficiency of rare earth nanoparticles is solved and near-term luminescence efficiency is achieved. The efficient conversion of infrared light into green and red light improves the photoelectric properties of the material.
Patent Information
- Application Number
- CN202311079613.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-08-25
AI Technical Summary
Rare earth upconversion nanoparticles have a single excitation wavelength and low upconversion luminescence efficiency, which limits their application in the fields of biological imaging, therapy, anti-counterfeiting coding, detection and photovoltaic devices, and the lattice mismatch in the composite heterojunction leads to Heterogeneous interface defects affect performance improvement.
By designing the BiOCl/BiOBr:Yb3+, Er3+ heterojunction structure with high lattice matching, the internal electric field characteristics of bismuth oxyhalide are used to enhance the luminescence of rare earth ions, increase the composite heterojunction interface electric field, and enhance the rare earth ion doping of bismuth oxyhalide. The luminescent properties of the material.
It achieves effective conversion of 980nm near-infrared light into 525nm and 554nm green light and 670nm red light, improves the photogenerated carrier separation efficiency and the luminescence performance of the material, and enhances the luminescence behavior of rare earth ions.
Smart Images

Figure CN117089347B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of up-conversion luminescent materials, and in particular relates to a heterojunction interface electric field enhanced up-conversion luminescent material and a preparation method thereof. Background Art
[0002] Rare earth-doped upconversion nanoparticles have been widely used in biological imaging and treatment, anti-counterfeiting coding, detection, photovoltaic devices and photocatalytic reactions due to their unique spectral properties, such as narrow-band emission under near-infrared excitation, large anti-Stokes shift, good optical stability and no biological background autofluorescence. However, the single excitation wavelength and low upconversion luminescence efficiency of rare earth upconversion nanoparticles limit their further practical application. In recent years, studies have found that by constructing composite heterojunctions and utilizing the energy level difference between composite materials and semiconductors of different components, the spectral absorption range can be effectively increased and the separation efficiency of photogenerated carrier pairs can be improved, thereby improving the photoelectric performance of the material. However, there is usually a large lattice mismatch between most composite heterojunctions, resulting in a large number of defects at the heterojunction interface, which becomes the recombination center of matrix carriers and the quenching center of rare earth ion luminescence, affecting the improvement of its performance.
[0003] Therefore, in order to solve the above problems, this paper proposes a heterojunction interface electric field enhanced up-conversion luminescent material and a preparation method thereof. Summary of the invention
[0004] In order to solve the above technical problems, the present invention designs a heterojunction interface electric field enhanced upconversion luminescent material and a preparation method thereof, which has a high lattice matching degree, reduces the crystal field around the rare earth ions, can enhance the luminescence of rare earth ions to a certain extent, and utilizes the internal electric field characteristics of bismuth halide oxide itself. The composite heterojunction interface electric field effectively enhances the luminescence behavior of rare earth ions, thereby improving the luminescence performance of rare earth ion-doped bismuth halide oxide materials.
[0005] In order to achieve the above technical effects, the present invention is implemented by the following technical scheme: a method for preparing a heterojunction upconversion light-emitting semiconductor nanomaterial, characterized in that it comprises the following steps:
[0006] Step 1: Dissolve the bismuth source and rare earth ion nitrate solution in mannitol solvent, stir and mix, then add the mixed solution containing bromine source, perform hydrothermal reaction on the obtained aqueous solution, centrifuge, wash, dry, and then anneal in air to obtain the first precursor BiOBr:Yb 3+ , Er 3+ ;
[0007] Step 2, dissolving the bismuth source in a mannitol solvent, stirring and mixing, and then adding an aqueous solution containing a chlorine source, subjecting the obtained mixed solution to a hydrothermal reaction, centrifuging, washing, drying, and then annealing in air to obtain a second precursor BiOCl;
[0008] Step 3, dissolving the first precursor and the second precursor in anhydrous ethanol solution for ultrasonic dispersion, stirring and mixing, drying, and annealing in air to obtain BiOCl / BiOBr:Yb 3+ , Er 3+ Heterojunction upconversion luminescent materials.
[0009] Furthermore, the bismuth source is bismuth nitrate pentahydrate or bismuth phosphate; the rare earth ion nitrate solution is Yb(NO 3 ) 3 Solution or Er(NO 3 ) 3 solution; the bromine source is sodium bromide or potassium bromide; the chlorine source is sodium chloride or potassium chloride.
[0010] Furthermore, the mass ratio of the bismuth source to the volume of the mannitol solution is 0.5-3 g: 20-50 mL;
[0011] The concentration of the rare earth ion aqueous solution is 0.1-4M;
[0012] The molar ratio of the bromine element in the bromine source to the bismuth element in the bismuth source is 0.5 to 5:1;
[0013] The molar ratio of the chlorine element in the chlorine source to the bismuth element in the bismuth source is 0.5-5:1.
[0014] Furthermore, the hydrothermal reaction temperature in Step 1 is 120-200° C., and the hydrothermal reaction time is 8-20 hours; the annealing temperature in Step 1 is 200-550° C., and the annealing time is 1-8 hours; the composite annealing temperature is 100-300° C., and the annealing time is 1-8 hours.
[0015] Furthermore, in Step 3, the mass ratio of the first precursor to the second precursor is 2:1.
[0016] Another object of the present invention is to provide a heterojunction upconversion light-emitting semiconductor nanomaterial, characterized in that its chemical formula is: BiOCl / BiOBr:Yb 3+ , Er 3+ .
[0017] The beneficial effects of the present invention are:
[0018] The nanomaterial of the present invention has the same Bi atoms and similar layered structures, and can not only form a stable composite heterostructure, but also generate oxygen vacancies at the composite interface to convert 980nm near-infrared light into 525nm and 554nm green light and 670nm red light, but also effectively promote the separation of photogenerated carriers through the energy level difference between BiOCl and BiOBr in the composite material to further enhance the luminescence performance of the material;
[0019] The nanomaterial of the present invention has a high lattice matching degree, reduces the crystal field around the rare earth ions, can enhance the luminescence of the rare earth ions to a certain extent, utilizes the internal electric field characteristics of the bismuth oxyhalide itself, and the composite heterojunction interface electric field effectively enhances the luminescence behavior of the rare earth ions, thereby improving the luminescence performance of the rare earth ion doped bismuth oxyhalide material. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0021] Figure 1 BiOCl / BiOBr:Yb prepared in Examples 1-3 of the present invention and Comparative Examples 1 and 2 3+ , Er 3+ X-ray diffraction patterns of composite materials;
[0022] Figure 2 BiOCl / BiOBr:Yb prepared in Examples 1-3 of the present invention and Comparative Examples 1 and 2 3+ , Er 3+ Scanning electron images of composite materials;
[0023] Figure 3 BiOCl / BiOBr:Yb prepared in Examples 1-3 of the present invention and Comparative Examples 1 and 2 3+ , Er 3+ Transmission electron microscopy images of the composite materials;
[0024] Figure 4 BiOCl / BiOBr:Yb prepared in Examples 1-3 of the present invention and Comparative Examples 1 and 2 3+ , Er 3+ Upconversion emission spectrum of the synthesized sample under 980nm excitation of the composite material. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] (1) Add 1mmol Bi(NO 3 ) 3 ·5H 2 O, 0.2mL Yb(NO 3 ) 3 (0.5mol / L), 0.1mL Er(NO 3 ) 3 (0.1mol / L) was dissolved in 20mL mannitol solution, and the mixed solution was stirred for 0.5h, then 0.5mmol NaBr solution was added and stirred for 10min. The above liquid was transferred to a 50mL reactor, placed in a 120℃ oven, kept for 8h, and then naturally cooled to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 550℃ in air atmosphere for 1h to obtain BiOBr:Yb 3+ , Er 3+ Nanosheets.
[0028] (2) 6mmol BiPO 4 Dissolve in 20 mL of mannitol solution, stir the mixed solution for 0.5 h, then add 2.5 mmol of NaCl solution and continue stirring for 10 min. Transfer the above liquid to a 50 mL reactor, place it in a 200 ° C oven, keep it for 20 h, and then cool it naturally to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450 ° C in air atmosphere for 2 h to obtain BiOCl microsheets.
[0029] (3) 0.6 g BiOBr:Yb 3+ , Er 3+ The nanosheets and 0.3 g BiOCl microsheets were ultrasonically dispersed in anhydrous ethanol, and then the two solutions were mixed, stirred and dried. The samples were collected and annealed in a muffle furnace at 200 °C in air for 3 h to obtain BiOCl / BiOBr:Yb 3+ , Er 3+ Composite materials. Figure 4 It can be seen that under 980nm excitation, BiOCl / BiOBr:Yb 3+ , Er 3+There are emission peaks at 525nm, 543nm and 672nm respectively, namely Er 3+ ion 2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 → 4 I 15 / 2 Green light from energy level transition and 4 F 9 / 2 → 4 I 15 / 2 Red light from energy level transition.
[0030] Example 2
[0031] (1) 3mmol BiPO 4 , 0.2mL Yb(NO 3 ) 3 (1 mol / L), 0.1 mL Er(NO 3 ) 3 (0.2mol / L) was dissolved in 20mL mannitol solution, and the mixed solution was stirred for 0.5h, then 0.5mmol NaBr solution was added and stirred for 10min. The above liquid was transferred to a 50mL reactor, placed in a 120℃ oven, kept for 8h, and then naturally cooled to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450℃ in air atmosphere for 1h to obtain BiOBr:Yb 3+ , Er 3+ Nanosheets.
[0032] (2) Add 6 mmol Bi(NO 3 ) 3 ·5H 2 O was dissolved in 20 mL of mannitol solution, and the mixed solution was stirred for 0.5 h, followed by the addition of 2.5 mmol of NaCl solution and continued stirring for 10 min. The above liquid was transferred to a 50 mL reactor, placed in a 160 ° C oven, kept for 12 h, and then naturally cooled to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450 ° C in an air atmosphere for 5 h to obtain BiOCl microsheets.
[0033] (3) 0.8 g BiOBr:Yb 3+ , Er 3+ The nanosheets and 0.4 g BiOCl microsheets were ultrasonically dispersed in anhydrous ethanol, and then the two solutions were mixed, stirred and dried. The obtained samples were collected and annealed in a muffle furnace at 250 °C in air atmosphere for 8 h to obtain BiOCl / BiOBr:Yb 3+, Er 3+ Composite materials. Figure 4 It can be seen that under 980nm excitation, BiOCl / BiOBr:Yb 3+ , Er 3+ There are emission peaks at 525nm, 543nm and 672nm respectively, namely Er 3+ ion 2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 → 4 I 15 / 2 Green light from energy level transition and 4 F 9 / 2 → 4 I 15 / 2 Red light from energy level transition.
[0034] Example 3
[0035] (1) 5 mmol BiPO 4 , 0.25mL Yb 2 O 3 (2mol / L), 0.5 mL Er 2 O 3 (0.1mol / L) was dissolved in 20mL mannitol solution, and the mixed solution was stirred for 0.5h, then 0.5mmol KBr solution was added and stirred for 10min. The above liquid was transferred to a 50mL reactor, placed in a 160℃ oven, kept for 12h, and then naturally cooled to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450℃ in air atmosphere for 8h to obtain BiOBr:Yb 3+ , Er 3+ Nanosheets.
[0036] (2) 5mmol BiPO 4 Dissolve in 20 mL of mannitol solution, stir the mixed solution for 0.5 h, then add 1 mmol of NaCl solution and continue stirring for 10 min. Transfer the above liquid to a 50 mL reactor, place it in an oven at 180 ° C, keep it for 12 h, and then cool it naturally to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450 ° C in air atmosphere for 2 h to obtain BiOCl micron sheets.
[0037] (3) 0.8 g BiOBr:Yb 3+ , Er 3+The nanosheets and 0.4 g BiOCl microsheets were ultrasonically dispersed in anhydrous ethanol, and then the two solutions were mixed, stirred and dried. The samples were collected and annealed in a muffle furnace at 200 °C in air for 5 h to obtain BiOCl / BiOBr:Yb 3+ , Er 3+ Composite materials. Figure 4 It can be seen that under 980nm excitation, BiOCl / BiOBr:Yb 3+ , Er 3+ There are emission peaks at 525nm, 543nm and 672nm respectively, namely Er 3+ ion 2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 → 4 I 15 / 2 Green light from energy level transition and 4 F 9 / 2 → 4 I 15 / 2 Red light from energy level transition.
[0038] Comparative Example 1
[0039] Add 5mmol Bi(NO 3 ) 3 ·5H 2 O, 1mL Yb(NO 3 ) 3 (0.5 mol / L), 0.5 mL Er(NO 3 ) 3 (0.1mol / L) was dissolved in 25mL mannitol solution, and the mixed solution was stirred for 0.5h, then 2mL KBr solution was added and stirred for 10min. The above liquid was transferred to a 50mL reactor, placed in a 160℃ oven, kept for 14h, and then naturally cooled to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450℃ in air atmosphere for 1h to obtain BiOBr:Yb 3 + ,Er 3+ Nanosheets. Figure 3 It can be seen that under 980nm excitation, BiOBr:Yb 3+ , Er 3+ There are emission peaks at 525nm, 543nm and 672nm respectively, namely Er 3+ ion 2 H 11 / 2 → 4 I 15 / 2 , 4 S3 / 2 → 4 I 15 / 2 Green light from energy level transition and 4 F 9 / 2 → 4 I 15 / 2 Compared with Example 1, the BiOBr:Yb 3+ , Er 3+ No heterojunction was formed with BiOCl, and the upconversion luminescence intensity was significantly lower than that of BiOCl / BiOBr:Yb in Example 1. 3+ , Er 3+ sample.
[0040] Comparative Example 2
[0041] (1) 3 mmol Bi(NO 3 ) 3 ·5H 2 O, 1mL Yb(NO 3 ) 3 (0.5 mol / L), 0.5 mL Er(NO 3 ) 3 (0.1mol / L) was dissolved in 25mL mannitol solution, and the mixed solution was stirred for 0.5h, then 2mmol KBr solution was added and stirred for 10min. The above liquid was transferred to a 50mL reactor, placed in a 160℃ oven, kept for 12h, and then naturally cooled to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450℃ air atmosphere for 2h to obtain BiOBr:Yb 3+ ,Er 3+ Nanosheets.
[0042] (2) Add 5mmol Bi(NO 3 ) 3 ·5H 2 O was dissolved in 25 mL of mannitol solution, and the mixed solution was stirred for 0.5 h, followed by the addition of 2 mmol of KCl solution and continued stirring for 10 min. The above liquid was transferred to a 50 mL reactor, placed in a 160 ° C oven, kept for 12 h, and then naturally cooled to room temperature. Finally, after centrifugal washing and drying, the sample was annealed in a muffle furnace at 450 ° C in an air atmosphere for 3 h to obtain BiOCl microsheets.
[0043] (3) 0.8 g BiOBr:Yb 3+ , Er 3+ The nanosheets and 0.4 g BiOCl microsheets were ultrasonically dispersed in anhydrous ethanol, and then the two solutions were mixed, stirred, and dried. The resulting sample was collected to obtain BiOCl / BiOBr:Yb3+ , Er 3 + Physically mix the sample. Figure 4 It can be seen that under 980nm excitation, BiOCl / BiOBr:Yb 3+ , Er 3+ The physical mixed sample has emission peaks at 525nm, 543nm and 672nm, namely Er 3+ ion 2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 → 4 I 15 / 2 Green light from energy level transition and 4 F 9 / 2 → 4 I 15 / 2 Compared with Example 1, the BiOCl / BiOBr:Yb 3+ , Er 3+ The upconversion luminescence performance of the physically mixed sample is weakened.
[0044] From Comparative Example 1, it can be seen that BiOCl has a significant effect on BiOBr:Yb 3+ , Er 3+ Nanocrystal modification can increase the 2 H 11 / 2 , 4 S 3 / 2 and 4 F 9 / 2 The electron population on the energy level can achieve upconversion luminescence enhancement. 3+ ,Er 3+ The energy level difference and the electric field at the interface can increase the – -h + For separation efficiency, increase the electrons in the conduction band to the adjacent Er 3+ The probability of ion energy level transfer effectively enhances the upconversion luminescence performance. 3+ , Er 3+ In the process of heterojunction formation, oxygen atoms are shared, and oxygen vacancies are generated at the composite interface as intermediate energy levels, which provide a bridge for the energy transfer process and effectively enhance the upconversion luminescence performance. At the same time, BiOCl and BiOBr:Yb 3+ , Er 3+ Has a high lattice matching degree, in BiOCl / BiOBr:Yb 3+ , Er 3+The formation of the heterojunction will reduce the crystal field around the rare earth ions and enhance the luminescence performance of the rare earth ions.
[0045] In summary, the present invention can prepare the upconversion luminescent BiOCl / BiOBr:Yb with heterostructure by hydrothermal method and annealing process. 3+ , Er 3+ Composite materials. The energy level difference and the oxygen vacancy energy level and internal electric field generated at the interface can improve the efficiency of photogenerated carrier separation and the ability of near-enhanced infrared light conversion to green and red light.
Claims
1. A method for preparing a heterojunction interface electric field enhanced upconversion luminescent material, characterized in that: The following steps are involved: Step 1: Dissolve the bismuth source and rare earth ion nitrate solution in mannitol solvent, stir and mix, then add the aqueous solution containing bromine source, perform hydrothermal reaction on the obtained mixed solution, centrifuge, wash, dry, and then anneal in air to obtain the first precursor BiOBr:Yb 3+ , Er 3+ ; Step 2, dissolving the bismuth source in a mannitol solvent, stirring and mixing, and then adding an aqueous solution containing a chlorine source, subjecting the obtained mixed solution to a hydrothermal reaction, centrifuging, washing, drying, and then annealing in air to obtain a second precursor BiOCl; Step 3, dissolving the first precursor and the second precursor in anhydrous ethanol solution for ultrasonic dispersion, stirring and mixing, drying, and annealing in air to obtain BiOCl / BiOBr:Yb 3+ , Er 3+ Heterojunction upconversion luminescent materials.
2. The method for preparing a heterojunction interface electric field enhanced up-conversion luminescent material according to claim 1, characterized in that: The bismuth source is bismuth nitrate pentahydrate or bismuth phosphate; the rare earth ion nitrate solution is Yb(NO3)3 solution or Er(NO3)3 solution; the bromine source is sodium bromide or potassium bromide; and the chlorine source is sodium chloride or potassium chloride.
3. The method for preparing a heterojunction interface electric field enhanced up-conversion luminescent material according to claim 2, characterized in that: The mass ratio of the bismuth source to the volume of the mannitol solution is 0.5-3 g: 20-50 mL; The concentration of the rare earth ion aqueous solution is 0.1-4M; The molar ratio of the bromine element in the bromine source to the bismuth element in the bismuth source is 0.5 to 5:1; The molar ratio of the chlorine element in the chlorine source to the bismuth element in the bismuth source is 0.5-5:
1.
4. The method for preparing a heterojunction interface electric field enhanced up-conversion luminescent material according to claim 1, characterized in that: The hydrothermal reaction temperature in Step 1 is 120-200° C., and the hydrothermal reaction time is 8-20 hours; the annealing temperature in Step 1 is 200-550° C., and the annealing time is 1-8 hours; the composite annealing temperature is 100-300° C., and the annealing time is 1-8 hours.
5. The method for preparing a heterojunction interface electric field enhanced up-conversion luminescent material according to claim 1, characterized in that: In the Step 3, the mass ratio of the first precursor to the second precursor is 2:
1.
6. The method for preparing a heterojunction interface electric field enhanced up-conversion luminescent material according to any one of claims 1 to 5, characterized in that: The chemical formula of a heterojunction interface electric field enhanced upconversion luminescent material is: BiOCl / BiOBr:Yb 3+ , Er 3+ .