By using modified coatings on composite floors, dopamine-modified graphene oxide and polysulfone particles are used to form a double-wall structure, which solves the problem of insufficient wear resistance and corrosion resistance of composite floor materials and achieves higher durability. Wear and corrosion resistance, and maintain environmentally friendly and healthy characteristics.

CN117124668BActive Publication Date: 2024-10-01HUIDONG MEIXIN PLASTIC LUMBER PROD MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311103739.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-30
Publication Date
2024-10-01
Estimated Expiration
2043-08-30

AI Technical Summary

Technical Problem

Existing composite flooring materials have poor wear resistance and corrosion resistance, and toxic substances are often used in traditional methods, which affects environmental protection.

Method used

A composite floor composed of medium density fiberboard, oak, maple, pine and other materials is used, and the surface is coated with a modified coating. The coating uses dopamine-modified graphene oxide and polysulfone particles to form a double-wall structure to enhance the thermal insulation of the coating. Stability and hydrophobicity, improve the wear resistance and corrosion resistance of the floor.

Benefits of technology

It significantly improves the wear resistance and corrosion resistance of the composite floor, enhances the mechanical and thermal properties of the coating, has self-healing and anti-corrosion functions, extends the service life of the floor, while maintaining environmentally friendly and healthy characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004421383830000131
    Figure BDA0004421383830000131
Patent Text Reader

Abstract

The present invention discloses a wear-resistant and corrosion-resistant composite floor material and a preparation method thereof. The composite floor material of the present invention is composed of a coating layer, a surface layer, a veneer layer, a core layer, and a back layer from top to bottom. A modified coating is coated on the upper surface of the surface layer, and the wear-resistant and corrosion-resistant composite floor material of the present invention is obtained by curing. Compared with the prior art, the composite floor material prepared by the present invention has the advantages of strong hydrophobicity, good wear resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite floor materials, and in particular to a wear-resistant and corrosion-resistant composite floor material and a preparation method thereof. Background Art

[0002] Common floor materials include: solid wood floor, laminate floor, special-shaped floor, stone floor, PVC floor, wood plastic floor, laboratory floor, etc. Laminated floor has the following advantages over traditional floor such as solid wood floor and tile floor: more affordable, compared with solid wood floor, laminate floor uses more diversified raw materials, more affordable, suitable for mass consumption. Stronger adaptability, laminate floor has stronger adaptability, not only can adapt to floor heating, but also can adapt to high humidity environment, not easy to deform, crack, etc. Convenient construction, laminate floor is simple and convenient to install, no need to apply putty, short installation cycle, and can be assembled without nails, no need to use glue and other materials, greatly reducing the construction difficulty and construction pollution. Easy maintenance, the surface of the laminate floor uses high-quality wear-resistant coating, with good waterproof, moisture-proof, anti-fouling and anti-scratch performance, usually only need to use mop and detergent for simple cleaning and maintenance. Environmentally friendly and healthy, the raw materials used in the laminate floor are added with environmentally friendly ingredients, non-toxic, odorless, not easy to release harmful substances such as formaldehyde, safer and healthier to use.

[0003] Composite flooring is a flooring made of multiple layers of materials, usually composed of the following layers: surface layer, veneer layer, core layer, and back layer. In the prior art, high-strength, high-wear-resistant surface materials such as high-density fiberboard (HDF), epoxy resin, aluminum oxide, etc. are usually used to improve the wear resistance of composite flooring. Surface coating is used to enhance the wear resistance of composite flooring. The floor is textured to increase the friction of the floor surface and improve the anti-slip and wear resistance of the floor. Common treatment methods include notching, embossing, and concave-convex. In the prior art, corrosion resistance is usually achieved by improving the surface coating. Common surface coatings include UV coatings, matte paint coatings, metal oxide coatings, etc. However, the above technologies have limited improvement in the wear resistance and corrosion resistance of composite flooring, and are also accompanied by the addition of some toxic substances, which is not environmentally friendly.

[0004] Invention patent application CN109109416A discloses a high-hardness wear-resistant composite floor and its preparation method, which solves the problems of low hardness, poor wear resistance, easy to be squeezed to cause depression, and easy to be scratched in the prior art. The high-hardness wear-resistant composite floor is formed by bonding a double-layer surface layer with a substrate layer in the middle, and the substrate layer is composed of a double-layer expandable polystyrene board with polyurethane in the middle; the surface layer includes the following raw materials: polyvinyl chloride, epoxy resin, 5-amino-6-methylbenzimidazolone, o-amino-tert-butylphenol, modifier, nano-silicon dioxide, aluminum oxide, glass wool, and additives. The composite floor prepared by the invention has high hardness, good mechanical properties, excellent wear resistance, flame retardancy, compression resistance, shock absorption, sound absorption, waterproof, antibacterial properties, and long service life. However, the wear resistance of the composite floor prepared by the invention is still poor, and the corrosion resistance needs to be improved. Summary of the invention

[0005] In view of the disadvantages of poor wear resistance and low corrosion resistance of the composite floor in the prior art, the technical problem to be solved by the present invention is to provide a composite floor material with good wear resistance and corrosion resistance and a preparation method thereof.

[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0007] The invention discloses a wear-resistant and corrosion-resistant composite floor material which is composed of a coating layer, a surface layer, a veneer layer, a core layer and a back layer from top to bottom.

[0008] Preferably, the surface layer is made of medium density fiberboard with a thickness of 1 to 5 mm.

[0009] The surface layer provides surface decoration and protection for the floor.

[0010] Preferably, the veneer layer is made of one of oak, maple or birch, and has a thickness of 3 to 6 mm.

[0011] Preferably, the core layer is made of pine or birch, and has a thickness of 3 to 8 mm.

[0012] Preferably, the back layer is one of paper or PE film.

[0013] The preparation method of the wear-resistant and corrosion-resistant composite floor material is as follows:

[0014] Step 1: The wear-resistant and corrosion-resistant composite floor material is composed of a coating layer, a surface layer, a veneer layer, a core layer, and a reverse layer from top to bottom. The adhesive layer is coated on the lower surface of the surface layer, and the adhesive layer is coated on the upper surface of the core layer. The adhesive layer is laminated on the lower surface of the surface layer and the adhesive layer is laminated on the upper surface of the core layer by a hot press at a temperature of 170 to 190° C., a pressure of 0.1 to 0.5 MPa, and a time of 5 to 20 minutes;

[0015] Step 2, placing a veneer layer between the adhesive layer composited with the surface layer and the adhesive layer composited with the core layer, and then impregnating the reverse layer with diallyl phthalate for 5 to 20 minutes, with the mass ratio of the reverse layer to diallyl phthalate being 1:5 to 15, and affixing it to the lower surface of the core layer, and using a hot press at a temperature of 170 to 190° C., a pressure of 1 to 3 MPa, and a time of 10 to 30 minutes, pressing it into one piece at one time;

[0016] Step 3: Apply the modified coating on the upper surface of the surface layer, and cure it at 60-90° C. for 20-50 minutes to obtain a coating with a thickness of 50-150 μm to obtain a wear-resistant and corrosion-resistant composite floor material.

[0017] Preferably, the adhesive layer is composed of silane coupling agent and plastic particles in a mass ratio of 3-5:4-8, and the coating amount of the adhesive layer is 50-150 g / m 2 .

[0018] The preparation method of the modified coating is as follows, in parts by weight:

[0019] S1. Adjust 150 to 250 parts of Tris-Triton-NaCl buffer to pH 8 to 9 with 0.05 to 0.2 mol / L hydrochloric acid to obtain a solvent to be used;

[0020] S2. Add 1 to 3 parts of polysulfone particles and 3 to 5 parts of oil to 80 to 120 parts of dichloromethane, stir at 100 to 500 rpm at room temperature for 1 to 3 hours to obtain an oil solution; add 8 to 12 parts of polyvinyl alcohol and 5 to 10 parts of gelatin to 80 to 120 parts of water, stir at 70 to 100° C. for 20 to 50 minutes at a stirring speed of 100 to 500 rpm to obtain an aqueous solution; drop the oil solution into the aqueous solution under stirring at 100 to 500 rpm at a dropping speed of 1 to 10 mL / min to obtain an emulsion;

[0021] S3, stirring the emulsion prepared in step S2 at 30-40°C at a speed of 200-1000 r / min for 1-3 h, then centrifuging at 10000-20000 rpm for 3-8 min, collecting the solid, washing it with water 1-3 times, and freeze-drying it at -10--40°C for 1-10 h to obtain a micro-solid;

[0022] S4, adding 0.2-0.6 parts of graphene oxide and 0.2-0.6 parts of dopamine to the standby solvent prepared in step S1, stirring at 100-600 rpm for 10-30 hours at room temperature, centrifuging at 10000-20000 rpm for multiple times until the pH of the upper solution is neutral, collecting the solid, and obtaining a composite;

[0023] S5. Add 1 to 3 parts of the microsolid prepared in step S3 and 0.4 to 0.6 parts of the complex prepared in step S4 to 800 to 1200 parts of a 1 to 3 mg / mL dopamine aqueous solution, stir at 100 to 500 rpm for 10 to 30 h at room temperature, wash with water 1 to 3 times, centrifuge at 12000 rpm for 3 to 8 min, collect the solid, and freeze-dry at -10 to -40°C for 1 to 10 h to obtain a modified compound;

[0024] S6. Add 0.4 to 0.6 parts of the modified compound prepared in step S5 to 4 to 6 parts of acetone, and then add to 5 to 12 parts of epoxy resin, stir at 100 to 600 rpm at room temperature for 0.5 to 2 hours, then add 4 to 8 parts of polyetheramine, and continue stirring at 100 to 600 rpm for 10 to 50 minutes to obtain a modified coating.

[0025] Preferably, the oil agent is one of white mineral oil, trimethylolpropane oleate, and hydroxystearate.

[0026] The composite floor material of the present invention is composed of a coating, a surface layer, a veneer layer, a core layer, and a back layer from top to bottom, and a modified coating is coated on the upper surface of the surface layer, and solidified to obtain the wear-resistant and corrosion-resistant composite floor material of the present invention. The modified coating is prepared by adjusting a Tris-Triton-NaCl buffer with hydrochloric acid to obtain a standby solvent; adding polysulfone particles and an oil agent to dichloromethane, stirring to obtain an oil solution, adding polyvinyl alcohol and gelatin to water, and stirring at high temperature to obtain an aqueous solution; adding the oil solution dropwise to the aqueous solution under stirring to obtain an emulsion; stirring the emulsion by centrifugation, washing and freeze-drying to obtain microsolids; adding graphene oxide and dopamine to the standby solvent, stirring and centrifuging to obtain a composite; adding microsolids and the composite to the dopamine aqueous solution, stirring and centrifuging, freeze-drying to obtain a modified compound; adding the modified compound to acetone, adding epoxy resin, and then adding polyetheramine, stirring to obtain the modified coating.

[0027] The active groups of dopamine, such as amine and hydroxyl groups, can form covalent bonds with oxygen-containing functional groups on the surface of inorganic or organic materials, thereby assembling graphene oxide on the surface of micro-solids to form a double-walled structure. The surface of the double-walled structure is a composite, and the interior is a microcapsule structure containing an oil agent. After graphene oxide is modified by dopamine, the thermal stability of the composite is improved, because dopamine forms a chemical bond, and the oxygen-containing groups of graphene oxide enhance the thermal stability of graphene oxide. The introduction of the composite further improves the thermal stability of the modified coating and can slow down the thermal decomposition of the modified coating, because the high rigidity of the composite limits the chain movement of the high-temperature softening polysulfone particles. In addition, after decomposition, the composite forms a carbon layer to protect the internal material and slow down the decomposition rate. In addition, the free radical scavenging ability of dopamine can eliminate the free radicals generated by the breakage of CC bonds, thereby preventing chain breakage and depolymerization. Therefore, the shell formed by the composite can protect the internal core and improve the overall thermal stability of the modified coating. Epoxy resin contains polar groups such as hydroxyl and ether bonds, which can form hydrogen bonds with the substrate, so that the coating has good physical adhesion properties. The functional groups contained in the composite can cross-link with the hydroxyl groups in the epoxy resin, further enhancing the interfacial bonding ability between the modified coating and the substrate. In addition, the rough shape of the double-walled structure surface increases its contact area with the substrate, further improving the interfacial compatibility of the coating.

[0028] The tribological properties of the composite flooring material were studied through friction and wear tests. The composite flooring material prepared by the present invention has excellent wear resistance for the following reasons. First, the composite material with a double-walled structure surface, as an excellent two-dimensional layered wear-resistant material, has an ultra-low friction coefficient itself and can fill the cavities and microcracks generated during sliding friction. Secondly, there are a large number of oxygen-containing functional groups on the surface of dopamine-modified graphene oxide, which can better combine with the epoxy resin matrix and play a wear-resistant role. Thirdly, when the modified coating is damaged, the oil with a low internal friction coefficient escapes to form a transfer film, which plays a synergistic lubricating role with graphene oxide. The wear debris of the modified coating fills the grooves. The worn surface of the modified coating becomes relatively smooth. The wear resistance of the composite flooring material is well improved.

[0029] Pure epoxy resin coatings are easily corroded by corrosive media due to their inherent brittleness and defects, so they have low corrosion resistance. After adding polysulfone particles, the pores generated after the epoxy resin is cured can be filled to a certain extent, making the coating structure dense. In addition, the white mineral oil in the modified coating can enhance the hydrophobicity of the coating surface, which is beneficial to blocking the penetration of corrosive media. In addition, the active groups of graphene oxide on the surface of the modified coating interact with the polar groups on the epoxy resin chain, which can improve the dispersibility and interfacial compatibility, thereby better utilizing the barrier and anti-corrosion effect of the epoxy resin matrix. During the corrosion process, due to the destruction of the modified coating, the oil agent is released from the damaged area. The released oil agent acts as a self-healing agent to self-heal the damaged area. Graphene oxide also has good barrier properties. The close interface bonding between dopamine-modified graphene oxide and the epoxy resin matrix inhibits the penetration of surface water molecules into the interior, and can form an effective barrier network, making the diffusion path of the corrosive medium more tortuous. This helps prevent corrosive media such as air, water, NaCl and acid and alkali from reaching the base of the composite floor material through the modified coating. In addition, the oil film in the modified coating combines with graphene oxide to form an insulating layer, which can inhibit the galvanic corrosion between graphene oxide and the composite floor material. Therefore, the modified coating can provide more lasting protection for the composite floor material.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1) The composite floor material of the present invention is composed of a coating layer, a surface layer, a veneer layer, a core layer, and a back layer from top to bottom. A modified coating is coated on the upper surface of the surface layer and cured to obtain the wear-resistant and corrosion-resistant composite floor material of the present invention. The prepared composite floor material has the advantages of strong hydrophobicity, good wear resistance and corrosion resistance.

[0032] 2) The present invention utilizes dopamine to assemble graphene oxide on the outer layer of polysulfone particles to prepare a modified compound, and fills it into epoxy resin to successfully prepare a modified coating, which improves the mechanical properties and thermal properties of the modified coating, and has good dispersibility and compatibility, and its adhesion strength, hardness and impact resistance are increased.

[0033] 3) The oil agent and graphene oxide flake layer in the present invention can play a synergistic lubricating role, the double-wall structure increases the corrosion path, and the prepared modified coating has a certain self-healing and anti-corrosion function. The self-healing property of this modified coating can be used to solve the wear and corrosion problems on the surface of composite floor materials. DETAILED DESCRIPTION

[0034] Main sources of substances:

[0035] Medium density fiberboard: Dongguan Fangjin Wood Industry Co., Ltd., item number: 21654948.

[0036] Silane coupling agent KH550: Shandong Hengyu New Materials Co., Ltd., model: KH550.

[0037] PVC plastic particles: Zhejiang Jinlida New Materials Technology Co., Ltd., brand: HA-1341.

[0038] Tris-Triton-NaCl buffer: Shanghai Huzhen Industrial Co., Ltd., pH: 9.0, product number: HZ-6020, purity: 99%.

[0039] Polysulfone particles: Shanghai Wenyan Plastics Co., Ltd., brand: P-1700.

[0040] White mineral oil: Suzhou Hesen Special Oil Co., Ltd., model: 5#, viscosity index: 121.

[0041] Polyvinyl alcohol: Zhengzhou Zhongyuan District Wanyuan Chemical Co., Ltd., model: 24-88.

[0042] Gelatin: Henan Pinman Food Co., Ltd., model: food grade, item number: 51 gelatin.

[0043] Dopamine: Merck, model: PHR1090-1G.

[0044] Polyetheramine: Guangzhou Kuibang Chemical Co., Ltd., model: 230.

[0045] PE film: Foshan Nanhai Yuanshen Plastic Factory, brand: A1552, thickness: 0.02mm.

[0046] Epoxy resin: Jinan Tengbo Chemical Co., Ltd., viscosity: 30mPas, product grade: industrial grade, model: E-44.

[0047] Graphene oxide: Zhejiang Zhiti Nano New Materials Co., Ltd., Features: multi-layer, fineness: 1~3nm.

[0048] Example 1

[0049] A wear-resistant and corrosion-resistant composite floor material, the preparation method is as follows:

[0050] Step 1: The wear-resistant and corrosion-resistant composite floor material is composed of a coating layer, a surface layer, a veneer layer, a core layer, and a reverse layer from top to bottom. The adhesive layer is applied on the lower surface of the surface layer. The surface layer is a medium-density fiberboard with a thickness of 2 mm. The upper surface of the core layer is coated with an adhesive layer. The core layer is birch with a thickness of 6 mm. The adhesive layer is composed of silane coupling agent KH550 and PVC plastic particles in a mass ratio of 4:6. The coating amount of the adhesive layer is 100 g / m 2, through a hot press: temperature 185°C, pressure 0.2MPa, time 10min, the lower surface of the surface layer is compounded with the adhesive layer, and the upper surface of the core layer is compounded with the adhesive layer;

[0051] Step 2, placing a veneer layer between the adhesive layer composited with the surface layer and the adhesive layer composited with the core layer, the veneer layer is made of oak and has a thickness of 4 mm, and then the reverse layer is impregnated with diallyl phthalate for 10 minutes, the mass ratio of the reverse layer to diallyl phthalate is 1:10, and is attached to the lower surface of the core layer. The reverse layer is a PE film, and a hot press is used at a temperature of 185°C, a pressure of 2.5MPa, and a time of 25 minutes to press it into one piece at one time;

[0052] Step 3: Apply the modified coating on the upper surface of the surface layer, and cure it at 80° C. for 45 minutes to obtain a coating with a thickness of 90 μm, thereby obtaining a wear-resistant and corrosion-resistant composite floor material.

[0053] The preparation method of the modified coating is as follows:

[0054] S1. Adjust 200 g Tris-Triton-NaCl buffer to pH 8.5 with 0.1 mol / L hydrochloric acid to obtain a solvent to be used;

[0055] S2. Add 2 g of polysulfone particles and 4 g of white mineral oil to 100 g of dichloromethane, stir at 200 rpm for 2 h at room temperature to obtain an oil solution; add 10 g of polyvinyl alcohol and 8 g of gelatin to 100 g of water, stir at 90 ° C for 40 min at a stirring speed of 300 rpm to obtain an aqueous solution; add the oil solution dropwise to the aqueous solution at a stirring speed of 5 mL / min at 200 rpm to obtain an emulsion;

[0056] S3, stirring the emulsion prepared in step S2 at 37° C. and 700 r / min for 2 h, then centrifuging at 12000 rpm for 5 min, collecting the solid, washing it with water for 3 times, and freeze-drying it at -20° C. for 5 h to obtain a micro-solid;

[0057] S4, adding 0.4 g of graphene oxide and 0.4 g of dopamine to the standby solvent prepared in step S1, stirring at 400 rpm for 24 h at room temperature, centrifuging at 12000 rpm for multiple times until the pH of the upper solution is neutral, collecting the solid, and obtaining a composite;

[0058] S5. Add 2 g of the microsolid prepared in step S3 and 0.5 g of the complex prepared in step S4 to 1000 g of a 2 mg / mL dopamine aqueous solution, stir at 350 rpm for 24 h at room temperature, wash twice with water, centrifuge at 12000 rpm for 5 min, collect the solid, and freeze-dry at -20°C for 5 h to obtain a modified compound;

[0059] S6. Add 0.5 g of the modified compound prepared in step S5 to 5 g of acetone, then add to 10 g of epoxy resin, stir at 400 rpm for 1 h at room temperature, then add 5.5 g of polyetheramine, and continue stirring at 400 rpm for 30 min to obtain a modified coating.

[0060] Example 2

[0061] The preparation method of a wear-resistant and corrosion-resistant composite floor material is basically the same as that of Example 1, with the only difference being that the preparation method of the modified coating is different.

[0062] The preparation method of the modified coating is as follows:

[0063] S1. Adjust 200 g Tris-Triton-NaCl buffer to pH 8.5 with 0.1 mol / L hydrochloric acid to obtain a solvent to be used;

[0064] S2. Add 4 g of white mineral oil to 100 g of dichloromethane, stir at 200 rpm for 2 h at room temperature to obtain an oil solution; add 10 g of polyvinyl alcohol and 8 g of gelatin to 100 g of water, stir at 90 ° C for 40 min at a stirring speed of 300 rpm to obtain an aqueous solution; add the oil solution dropwise to the aqueous solution at a stirring speed of 5 mL / min at 200 rpm to obtain a mixed solution;

[0065] S3, stirring the mixed solution prepared in step S2 at 37° C. and 700 r / min for 2 h, then evaporating the solvent in a 100° C. water bath, collecting the solid, washing it with water for 3 times, and freeze-drying it at -20° C. for 5 h to obtain a micro-solid;

[0066] S4, adding 0.4 g of graphene oxide and 0.4 g of dopamine to the standby solvent prepared in step S1, stirring at 400 rpm for 24 h at room temperature, centrifuging at 12000 rpm for multiple times until the pH of the upper solution is neutral, collecting the solid, and obtaining a composite;

[0067] S5. Add 2 g of the microsolid prepared in step S3 and 0.5 g of the complex prepared in step S4 to 1000 g of a 2 mg / mL dopamine aqueous solution, stir at 350 rpm for 24 h at room temperature, wash twice with water, centrifuge at 12000 rpm for 5 min, collect the solid, and freeze-dry at -20°C for 5 h to obtain a modified compound;

[0068] S6. Add 0.5 g of the modified compound prepared in step S5 to 5 g of acetone, then add to 10 g of epoxy resin, stir at 400 rpm for 1 h at room temperature, then add 5.5 g of polyetheramine, and continue stirring at 400 rpm for 30 min to obtain a modified coating.

[0069] Example 3

[0070] The preparation method of a wear-resistant and corrosion-resistant composite floor material is basically the same as that of Example 1, with the only difference being that the preparation method of the modified coating is different.

[0071] The preparation method of the modified coating is as follows:

[0072] S1. Adjust 200 g Tris-Triton-NaCl buffer to pH 8.5 with 0.1 mol / L hydrochloric acid to obtain a solvent to be used;

[0073] S2. Add 2 g of polysulfone particles to 100 g of dichloromethane, stir at 200 rpm for 2 h at room temperature to obtain a polysulfone solution; add 10 g of polyvinyl alcohol and 8 g of gelatin to 100 g of water, stir at 90 ° C for 40 min at a stirring speed of 300 rpm to obtain an aqueous solution; add the polysulfone solution dropwise to the aqueous solution at a stirring speed of 5 mL / min at 200 rpm to obtain an emulsion;

[0074] S3, stirring the emulsion prepared in step S2 at 37° C. and 700 r / min for 2 h, then centrifuging at 12000 rpm for 5 min, collecting the solid, washing it with water for 3 times, and freeze-drying it at -20° C. for 5 h to obtain a micro-solid;

[0075] S4, adding 0.4 g of graphene oxide and 0.4 g of dopamine to the standby solvent prepared in step S1, stirring at 400 rpm for 24 h at room temperature, centrifuging at 12000 rpm for multiple times until the pH of the upper solution is neutral, collecting the solid, and obtaining a composite;

[0076] S5. Add 2 g of the microsolid prepared in step S3 and 0.5 g of the complex prepared in step S4 to 1000 g of a 2 mg / mL dopamine aqueous solution, stir at 350 rpm for 24 h at room temperature, wash twice with water, centrifuge at 12000 rpm for 5 min, collect the solid, and freeze-dry at -20°C for 5 h to obtain a modified compound;

[0077] S6. Add 0.5 g of the modified compound prepared in step S5 to 5 g of acetone, then add to 10 g of epoxy resin, stir at 400 rpm for 1 h at room temperature, then add 5.5 g of polyetheramine, and continue stirring at 400 rpm for 30 min to obtain a modified coating.

[0078] Example 4

[0079] The preparation method of a wear-resistant and corrosion-resistant composite floor material is basically the same as that of Example 1, with the only difference being that the preparation method of the modified coating is different.

[0080] The preparation method of the modified coating is as follows:

[0081] S1. Adjust 200 g Tris-Triton-NaCl buffer to pH 8.5 with 0.1 mol / L hydrochloric acid to obtain a solvent to be used;

[0082] S2, add 2g of polysulfone particles and 4g of white mineral oil to 100g of dichloromethane, stir at 200rpm for 2h at room temperature to obtain an oil solution, add 10g of polyvinyl alcohol and 8g of gelatin to 100g of water, stir at 90°C for 40min at a stirring speed of 300rpm to obtain an aqueous solution; add the oil solution dropwise to the aqueous solution at a stirring speed of 5mL / min at 200rpm to obtain an emulsion;

[0083] S3, stirring the emulsion prepared in step S2 at 37° C. and 700 r / min for 2 h, then centrifuging at 12000 rpm for 5 min, collecting the solid, washing it with water for 3 times, and freeze-drying it at -20° C. for 5 h to obtain a micro-solid;

[0084] S4, adding 2 g of the micro-solid prepared in step S3 to 1000 g of 2 mg / mL dopamine aqueous solution, stirring at 350 rpm for 24 h at room temperature, washing twice with water, centrifuging at 12000 rpm for 5 min, collecting the solid, and freeze-drying at -20°C for 5 h to obtain a modified compound;

[0085] S5. Add 0.5 g of the modified compound prepared in step S4 to 5 g of acetone, then add to 10 g of epoxy resin, stir at 400 rpm for 1 h at room temperature, then add 5.5 g of polyetheramine, and continue stirring at 400 rpm for 30 min to obtain a modified coating.

[0086] Comparative Example 1

[0087] The preparation method of a wear-resistant and corrosion-resistant composite floor material is basically the same as that of Example 1, with the only difference being that the preparation method of the modified coating is different.

[0088] The preparation method of the modified coating is as follows:

[0089] S1. Adjust 200 g Tris-Triton-NaCl buffer to pH 8.5 with 0.1 mol / L hydrochloric acid to obtain a solvent to be used;

[0090] S2. Add 10 g of polyvinyl alcohol and 8 g of gelatin to 100 g of water, stir at 90° C. for 40 min at a stirring speed of 300 rpm to obtain an aqueous solution; add 100 g of dichloromethane dropwise to the aqueous solution at a stirring speed of 5 mL / min at 200 rpm to obtain a mixed solution;

[0091] S3, stirring the mixed solution prepared in step S2 at 37° C. and 700 r / min for 2 h, then evaporating the solvent in a 100° C. water bath, collecting the solid, washing it with water for 3 times, and freeze-drying it at -20° C. for 5 h to obtain a micro-solid;

[0092] S4, adding 2 g of the micro-solid prepared in step S3 to 1000 g of 2 mg / mL dopamine aqueous solution, stirring at 350 rpm for 24 h at room temperature, washing twice with water, centrifuging at 12000 rpm for 5 min, collecting the solid, and freeze-drying at -20°C for 5 h to obtain a modified compound;

[0093] S5. Add 0.5 g of the modified compound prepared in step S4 to 5 g of acetone, then add to 10 g of epoxy resin, stir at 400 rpm for 1 h at room temperature, then add 5.5 g of polyetheramine, and continue stirring at 400 rpm for 30 min to obtain a modified coating.

[0094] Comparative Example 2

[0095] The preparation method of a wear-resistant and corrosion-resistant composite floor material is basically the same as that of Example 1, with the only difference being that the modified coating used in step 3 is replaced by an equal amount of epoxy resin.

[0096] Test Example 1

[0097] Wear resistance test

[0098] The wear resistance of the wear-resistant and corrosion-resistant composite floor prepared by the present invention was tested by using a JM-IV abrasion tester and a rotating friction rubber wheel method. The wear resistance of the present invention was measured by the average value of the coating mass loss (weight loss method) after 100 grinding revolutions. The load was 10N, the rotation speed was 80r / min, the test temperature was 25°C, the relative humidity was 50%, the mass was tested to an accuracy of 0.01mg, and the average value of 3 measurements was taken as the result. The test results are shown in Table 1.

[0099] Table 1: Wear resistance test results

[0100] Trial plan 100 revolutions mass loss / mg Example 1 42.61 Example 2 58.49 Example 3 59.02 Example 4 61.83 Comparative Example 1 97.48 Comparative Example 2 163.62

[0101] Test Example 2

[0102] Corrosion resistance test

[0103] The wear-resistant and corrosion-resistant composite floor prepared by the present invention was subjected to a corrosion resistance test.

[0104] Water resistance test: Add deionized water into a glass tank, adjust the water temperature to 40±1℃, and maintain this temperature during the whole process. Put three test panels into it, and immerse 2 / 3 of the length of the test panels in water. After 240 hours, take out the test panels, absorb the moisture with filter paper, observe and record whether one side of the coating has loss of gloss, discoloration, bubbles, wrinkles, shedding, etc.

[0105] Salt resistance test: The wear-resistant and corrosion-resistant composite floor prepared by the present invention is dried for 48 hours under constant temperature and humidity conditions. Sodium chloride is prepared into a 3% aqueous solution by mass with distilled water, and two-thirds of the composite floor is immersed in the salt solution at a temperature of 25±1°C. After 240 hours, the sample is taken out, the salt traces are washed off with water, and the water is dried with filter paper. Observe whether one side of the coating has peeling, wrinkling, bubbles, rust, discoloration, loss of gloss, etc.

[0106] Acid resistance test: The wear-resistant and corrosion-resistant composite floor prepared by the present invention is dried under constant temperature and humidity conditions for 48 hours. Two-thirds of the composite floor is immersed in 5% hydrochloric acid for 48 hours, then taken out, washed with water, and dried with filter paper. Observe whether one side of the coating has gloss loss, discoloration, bubbles, spots, shedding, etc.

[0107] Alkali resistance test: The wear-resistant and corrosion-resistant composite floor prepared by the present invention is dried under constant temperature and humidity conditions for 48 hours. Two-thirds of the composite floor is immersed in a 5% sodium hydroxide aqueous solution for 48 hours, then taken out, washed with water, and dried with filter paper. Observe whether one side of the coating has gloss loss, discoloration, bubbles, spots, shedding, etc.

[0108] Each sample was tested 5 times. The phenomenon with the highest frequency was selected and the test results are shown in Table 2.

[0109] Table 2: Corrosion resistance test results

[0110]

[0111] The degree of corrosion from large to small: a large number of bubbles, partial detachment > a small number of bubbles, a small number of spots > a large amount of gloss loss, severe discoloration > a small amount of gloss loss, slight discoloration > a very small amount of gloss loss, no discoloration > no gloss loss, no discoloration.

[0112] It can be seen from the test results of test examples 1 and 2 that the wear resistance and corrosion resistance of embodiment 1 are the best. The possible reason is that the present invention uses dopamine to assemble graphene oxide in the outer layer of polysulfone particles to prepare a modified compound, and fills it into epoxy resin to successfully prepare a modified coating. The surface of the prepared modified coating is rough, and the surface is a dopamine-modified graphene oxide adhesion layer, forming a double-walled structure. Since the amino group of dopamine forms a chemical bond with the oxygen-containing functional groups of graphene oxide and epoxy resin, the mechanical properties and thermal properties of the modified coating are improved. The dispersibility and compatibility of the modified coating are enhanced, and its adhesion strength, hardness and impact resistance are increased. Compared with pure epoxy resin coating, the wear resistance of the prepared modified coating is increased, and the surface hydrophobicity is enhanced. It also shows excellent self-healing anti-corrosion function. White mineral oil and graphene oxide flakes play a synergistic lubrication role, and the double-walled structure increases the corrosion path. In addition, the white mineral oil in the modified coating is released to form a repair film, which increases the hydrophobicity of the coating surface and further blocks the invasion of corrosive media, thereby achieving self-healing corrosion protection. This modified coating self-healing coating can be used to solve the wear and corrosion problems on the surface of composite floor materials.

Claims

1. A wear-resistant and corrosion-resistant composite floor material, characterized in that: From top to bottom, it consists of coating layer, surface layer, veneer layer, core layer and back layer; The surface layer is made of medium density fiberboard with a thickness of 1-5 mm; The veneer layer is one of oak, maple or birch, with a thickness of 3-6 mm; The core layer is one of pine and birch, with a thickness of 3-8 mm; The reverse layer is one of paper or PE film; The preparation steps of the wear-resistant and corrosion-resistant composite floor material are as follows: Step 1: The wear-resistant and corrosion-resistant composite floor material is composed of a coating layer, a surface layer, a veneer layer, a core layer, and a reverse layer from top to bottom. First, an adhesive layer is applied on the lower surface of the surface layer, and an adhesive layer is applied on the upper surface of the core layer. The adhesive layer is applied on the lower surface of the surface layer and the adhesive layer is applied on the upper surface of the core layer. The adhesive layer is applied on the lower surface of the surface layer and the adhesive layer is applied on the upper surface of the core layer by a hot press at a temperature of 170-190° C., a pressure of 0.1-0.5 MPa, and a time of 5-20 min. Step 2, placing a veneer layer between the adhesive layer composited with the surface layer and the adhesive layer composited with the core layer, and then impregnating the reverse layer with diallyl phthalate for 5 to 20 minutes, with the mass ratio of the reverse layer to diallyl phthalate being 1:5 to 15, and affixing it to the lower surface of the core layer, and using a hot press at a temperature of 170 to 190° C., a pressure of 1 to 3 MPa, and a time of 10 to 30 minutes, pressing it into one piece at one time; Step 3: coating the modified coating on the upper surface of the surface layer, curing at 60-90° C. for 20-50 min to obtain a coating with a thickness of 50-150 μm, and obtaining a wear-resistant and corrosion-resistant composite floor material; The adhesive layer is composed of silane coupling agent and plastic particles in a mass ratio of 3-5:4-8, and the coating amount of the adhesive layer is 50-150g / m 2 ; The preparation method of the modified coating is as follows, in parts by weight: S1. Adjust 150-250 parts of Tris-Triton-NaCl buffer to pH 8-9 with 0.05-0.2 mol / L hydrochloric acid to obtain a solvent for use; S2. Add 1 to 3 parts of polysulfone particles and 3 to 5 parts of oil to 80 to 120 parts of dichloromethane, stir at 100 to 500 rpm at room temperature for 1 to 3 hours to obtain an oil solution; add 8 to 12 parts of polyvinyl alcohol and 5 to 10 parts of gelatin to 80 to 120 parts of water, stir at 70 to 100° C. for 20 to 50 minutes at a stirring speed of 100 to 500 rpm to obtain an aqueous solution; dropwise add the oil solution to the aqueous solution under stirring at 100 to 500 rpm at a dropping speed of 1 to 10 mL / min to obtain an emulsion; S3, stirring the emulsion prepared in step S2 at 30-40°C at a speed of 200-1000 r / min for 1-3 h, then centrifuging at 10000-20000 rpm for 3-8 min, collecting the solid, washing it with water 1-3 times, and freeze-drying it at -10--40°C for 1-10 h to obtain a micro-solid; S4, adding 0.2-0.6 parts of graphene oxide and 0.2-0.6 parts of dopamine to the standby solvent prepared in step S1, stirring at 100-600 rpm for 10-30 hours at room temperature, centrifuging at 10000-20000 rpm for multiple times until the pH of the upper solution is neutral, collecting the solid, and obtaining a composite; S5. Add 1 to 3 parts of the microsolid prepared in step S3 and 0.4 to 0.6 parts of the complex prepared in step S4 to 800 to 1200 parts of a 1 to 3 mg / mL dopamine aqueous solution, stir at 100 to 500 rpm for 10 to 30 h at room temperature, wash with water 1 to 3 times, centrifuge at 12000 rpm for 3 to 8 min, collect the solid, and freeze-dry at -10 to -40°C for 1 to 10 h to obtain a modified compound; S6. Add 0.4-0.6 parts of the modified compound prepared in step S5 to 4-6 parts of acetone, and then add to 5-12 parts of epoxy resin, stir at 100-600 rpm at room temperature for 0.5-2 hours, then add 4-8 parts of polyetheramine, and continue stirring at 100-600 rpm for 10-50 minutes to obtain a modified coating.

2. The wear-resistant and corrosion-resistant composite floor material according to claim 1, characterized in that: The oil agent is one of white mineral oil, trimethylolpropane oleate and hydroxystearate.