A modified composite epoxy asphalt mixture and pavement construction method and equipment

By using high-toughness polyurethane modified epoxy resin and SK-70 matrix asphalt and other raw materials to prepare modified composite epoxy asphalt mixture, the problem of poor toughness of epoxy resin under low temperature conditions is solved, and its cracking resistance is improved. Paved on steel bridge.

CN117126545BActive Publication Date: 2024-10-22CHONGQING SINCERE BOND PAVEMENT MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311028744.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-16
Publication Date
2024-10-22
Estimated Expiration
2043-08-16

AI Technical Summary

Technical Problem

Epoxy resin has poor toughness and high brittleness under low temperature conditions, which affects its application in steel bridge paving.

Method used

Using raw materials such as high-toughness polyurethane modified epoxy resin and SK-70 matrix asphalt, a modified composite epoxy asphalt mixture is prepared through a specific molar ratio and a heating and stirring process to improve its cracking resistance.

Benefits of technology

It significantly improves the cracking resistance of the mixture, solves the problem of poor toughness of epoxy resin under low temperature conditions, and is suitable for steel bridge paving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117126545B_ABST
    Figure CN117126545B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of asphalt, and in particular to a modified composite epoxy asphalt mixture and a pavement construction method and equipment. The modified composite epoxy asphalt mixture is prepared by using the following raw materials in parts by weight: 35-45% of high-toughness polyurethane modified epoxy resin, 1-2% of curing agent, 2-4% of compatibilizer and 50-65% of SK-70 matrix asphalt, thereby improving the crack resistance of the mixture and solving the problem that the epoxy resin has the disadvantages of poor toughness and large brittleness under low temperature conditions; the curing agent, the compatibilizer and the SK-70 matrix asphalt are added into a disassembly barrel, and heated and stirred at a temperature of 100-140 DEG C, and then the high-toughness polyurethane modified epoxy resin is added, and the modified composite epoxy asphalt binder is obtained after uniform stirring. After the modified composite epoxy asphalt mixture is prepared, the disassembly barrel can be taken out from the inside of a box body to clean the disassembly barrel, thereby solving the problem of inconvenient cleaning of the inner wall of the box body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of asphalt, and in particular to a modified composite epoxy asphalt mixture and a pavement construction method and equipment. Background Art

[0002] Epoxy asphalt mixture is a thermosetting material, which is very important in steel bridge paving. It has good mechanical properties, fatigue resistance and high temperature stability, especially good load deformation resistance at high temperature, and is widely used in beam bridge deck paving.

[0003] However, since epoxy asphalt is modified with thermosetting epoxy resin, compared with asphalt materials, epoxy resin has the disadvantages of poor toughness and high brittleness under low temperature conditions. Summary of the invention

[0004] The purpose of the present invention is to provide a modified composite epoxy asphalt mixture and a pavement construction method and equipment, which improve the crack resistance of the mixture and solve the problem that epoxy resin has poor toughness and high brittleness under low temperature conditions.

[0005] To achieve the above-mentioned purpose, the present invention provides a modified composite epoxy asphalt mixture, which is prepared by using the following raw materials in the following weight ratio: 35-45% of high-toughness polyurethane modified epoxy resin, 1-2% of curing agent, 2-4% of compatibilizer and 50-65% of SK-70 base asphalt.

[0006] The high-toughness polyurethane modified epoxy resin is prepared from polyether diol, dicyclohexylmethane diisocyanate and epoxy resin in a molar ratio of 0.8-1.2: 2.0-2.6: 1.8-2.2.

[0007] Wherein, the preparation process of the high-toughness polyurethane modified epoxy resin is:

[0008] Weigh polyether diol, dicyclohexylmethane diisocyanate and epoxy resin in order according to a molar ratio of 0.8-1.2:2.0-2.6:1.8-2.2;

[0009] The polyether diol reacts with dicyclohexylmethane diisocyanate to form a polyurethane prepolymer terminated with an isocyanate group;

[0010] The polyurethane prepolymer is reacted with the epoxy resin to synthesize the high-toughness polyurethane modified epoxy resin.

[0011] Wherein, the preparation process of the modified composite epoxy asphalt mixture is:

[0012] The curing agent, the compatibilizer and the SK-70 base asphalt are heated and melted at a temperature of 100 to 140° C. to obtain a mixture;

[0013] The high-toughness polyurethane modified epoxy resin is heated at a temperature of 100 to 140° C., and added to the mixture for stirring, and after stirring evenly, a modified composite epoxy asphalt binder is obtained;

[0014] Add the modified composite epoxy asphalt binder to the aggregate with a petroleum ratio of 6 to 8%, mix well and then discharge;

[0015] The mixture is cured at a temperature of 120 to 130°C for 3 to 4 hours, and then solidified to obtain a modified composite epoxy asphalt mixture.

[0016] The present invention also provides a pavement construction method for the modified composite epoxy asphalt mixture described above, which specifically comprises the following steps:

[0017] Set the base by laying out lines and leveling;

[0018] Providing a thermal insulation layer on the base layer and laying a concrete sub-layer on the thermal insulation layer;

[0019] Laying epoxy asphalt waterproof bonding layer on the concrete base;

[0020] A modified composite epoxy asphalt mixture layer is laid on the waterproof bonding layer.

[0021] The present invention also provides an apparatus for preparing the modified composite epoxy asphalt mixture described above, comprising a box body, a heating plate, an agitator, a box cover and a disassembly cylinder, wherein the heating plate is arranged at the inner bottom of the box body, the box cover is detachably connected to the box body, the box cover is located above the box body, the agitator is arranged below the box cover, the disassembly cylinder is detachably connected to the box body, and the disassembly cylinder is located on the inner side of the box body.

[0022] The modified composite epoxy asphalt mixture and the pavement construction method and equipment of the present invention are prepared by using the following raw materials in parts by weight: 35-45% of high-toughness polyurethane modified epoxy resin, 1-2% of curing agent, 2-4% of compatibilizer and 50-65% of SK-70 matrix asphalt, which improves the crack resistance of the mixture and solves the problem that the epoxy resin has poor toughness and high brittleness under low temperature conditions. When preparing the modified composite epoxy asphalt mixture, firstly put the high-toughness polyurethane modified epoxy resin into the disassembly barrel, heat it to 100-140°C through the heating plate and then take it out, then add the curing agent, compatibilizer and SK-70 matrix asphalt into the disassembly barrel, heat and stir it at a temperature of 100-140°C to obtain a mixture, then add the heated high-toughness polyurethane modified epoxy resin, stir it evenly to obtain the modified composite epoxy asphalt binder, then add the modified composite epoxy asphalt binder to the aggregate with a petroleum ratio of 6-8%, stir it evenly and then discharge it; maintain it at a temperature of 120-130°C for 3-4h, and obtain the modified composite epoxy asphalt mixture after curing. After preparing the modified composite epoxy asphalt mixture, the disassembly barrel can be taken out from the inside of the box to clean the disassembly barrel, thereby solving the problem of inconvenient cleaning of the inner wall of the box. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0024] Figure 1 The present invention is a flow chart for preparing a high-toughness polyurethane modified epoxy resin for a modified composite epoxy asphalt mixture.

[0025] Figure 2 The present invention is a preparation flow chart of a modified composite epoxy asphalt mixture.

[0026] Figure 3 The present invention is a flow chart of a pavement construction method for modified composite epoxy asphalt mixture.

[0027] Figure 4 The present invention is a structural cross-sectional view of a device for preparing a modified composite epoxy asphalt mixture.

[0028] Figure 5 The present invention Figure 4 Cross-sectional view at AA in the middle.

[0029] 101-box body, 102-heating plate, 103-agitator, 104-box cover, 105-disassembly cylinder, 106-positioning bracket, 107-positioning groove, 108-discharging cylinder, 109-discharging port, 110-blocking column, 111-connecting ring. DETAILED DESCRIPTION

[0030] Embodiments of the present invention are described in detail below. Examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0031] See also Figure 1 and Figure 2 , Figure 1 This is a flow chart of the preparation of a high-toughness polyurethane-modified epoxy resin for a modified composite epoxy asphalt mixture of the present invention. Figure 2 The present invention provides a modified composite epoxy asphalt mixture, which is prepared by using the following raw materials in weight ratio: 35-45% of high-toughness polyurethane modified epoxy resin, 1-2% of curing agent, 2-4% of compatibilizer and 50-65% of SK-70 matrix asphalt.

[0032] Specifically, the high-toughness polyurethane modified epoxy resin is prepared from polyether diol, dicyclohexylmethane diisocyanate, and epoxy resin in a molar ratio of 0.8-1.2: 2.0-2.6: 1.8-2.2.

[0033] The preparation process of the high-toughness polyurethane modified epoxy resin is as follows:

[0034] S101: weigh polyether diol, dicyclohexylmethane diisocyanate and epoxy resin in sequence according to a molar ratio of 0.8-1.2:2.0-2.6:1.8-2.2;

[0035] S102: polyether diol reacts with dicyclohexylmethane diisocyanate to generate a polyurethane prepolymer terminated with an isocyanate group;

[0036] S103: reacting the polyurethane prepolymer with the epoxy resin to synthesize a high-toughness polyurethane-modified epoxy resin.

[0037] The preparation process of the modified composite epoxy asphalt mixture is as follows:

[0038] S201: heating and melting the curing agent, the compatibilizer and the SK-70 base asphalt at a temperature of 100 to 140° C. to obtain a mixture;

[0039] S202: heating a high-toughness polyurethane modified epoxy resin at a temperature of 100 to 140° C., adding the resin to the mixture and stirring the mixture, and obtaining a modified composite epoxy asphalt binder after stirring the mixture evenly;

[0040] S203: adding the modified composite epoxy asphalt binder to the aggregate with a petroleum ratio of 6 to 8%, stirring evenly and then discharging the material;

[0041] S204: Curing at a temperature of 120-130°C for 3-4 hours to obtain a modified composite epoxy asphalt mixture after solidification.

[0042] Example 1

[0043] Preparation of high-toughness polyurethane modified epoxy resin: weigh polyether diol, dicyclohexylmethane diisocyanate and epoxy resin in sequence according to a molar ratio of 0.8:2.0:2.2; react the polyether diol with dicyclohexylmethane diisocyanate to generate a polyurethane prepolymer terminated with an isocyanate group; react the polyurethane prepolymer with the epoxy resin to synthesize a high-toughness polyurethane modified epoxy resin.

[0044] Preparation of modified composite epoxy asphalt mixture: heating and melting a curing agent, a compatibilizer and SK-70 matrix asphalt at 140°C to obtain a mixture; heating a high-toughness polyurethane modified epoxy resin at 100°C, adding the resin to the mixture and stirring it, and obtaining a modified composite epoxy asphalt binder after uniform stirring; adding the modified composite epoxy asphalt binder to aggregates with a petroleum ratio of 6%, stirring the mixture and discharging the mixture; curing the mixture at 120°C for 3 hours, and obtaining a modified composite epoxy asphalt mixture after solidification.

[0045] Example 2

[0046] Preparation of high-toughness polyurethane modified epoxy resin: weigh polyether diol, dicyclohexylmethane diisocyanate and epoxy resin in sequence according to a molar ratio of 1.0:2.02:1.8; react the polyether diol with dicyclohexylmethane diisocyanate to generate a polyurethane prepolymer terminated with an isocyanate group; react the polyurethane prepolymer with the epoxy resin to synthesize a high-toughness polyurethane modified epoxy resin.

[0047] Preparation of modified composite epoxy asphalt mixture: heating and melting the curing agent, compatibilizer and SK-70 matrix asphalt at 110°C to obtain a mixture; heating high-toughness polyurethane modified epoxy resin at 110°C, adding it to the mixture and stirring it, and obtaining a modified composite epoxy asphalt binder after stirring evenly; adding the modified composite epoxy asphalt binder to aggregates with a petroleum ratio of 7%, stirring evenly and discharging the materials; curing at 125°C for 4 hours, and obtaining a modified composite epoxy asphalt mixture after curing.

[0048] Example 3

[0049] Preparation of high-toughness polyurethane modified epoxy resin: weigh polyether diol, dicyclohexylmethane diisocyanate and epoxy resin in sequence at a molar ratio of 1.2:2.0:2.0; react the polyether diol with dicyclohexylmethane diisocyanate to generate a polyurethane prepolymer terminated with an isocyanate group; react the polyurethane prepolymer with the epoxy resin to synthesize a high-toughness polyurethane modified epoxy resin.

[0050] Preparation of modified composite epoxy asphalt mixture: heating and melting the curing agent, compatibilizer and SK-70 matrix asphalt at 120°C to obtain a mixture; heating high-toughness polyurethane modified epoxy resin at 120°C, adding it to the mixture and stirring it, and obtaining a modified composite epoxy asphalt binder after stirring evenly; adding the modified composite epoxy asphalt binder to aggregates with a petroleum ratio of 7%, stirring evenly and discharging the materials; curing at 130°C for 3.5 hours, and obtaining a modified composite epoxy asphalt mixture after curing.

[0051] Example 4

[0052] Preparation of high-toughness polyurethane modified epoxy resin: weigh polyether diol, dicyclohexylmethane diisocyanate and epoxy resin in sequence according to the molar ratio of 0.8-1.2:2.0-2.6:1.8-2.2; react the polyether diol with dicyclohexylmethane diisocyanate to generate a polyurethane prepolymer terminated with an isocyanate group; react the polyurethane prepolymer with the epoxy resin to synthesize the high-toughness polyurethane modified epoxy resin.

[0053] Preparation of modified composite epoxy asphalt mixture: heating and melting a curing agent, a compatibilizer and SK-70 matrix asphalt at 130°C to obtain a mixture; heating a high-toughness polyurethane modified epoxy resin at 140°C, adding the resin to the mixture and stirring it, and obtaining a modified composite epoxy asphalt binder after stirring evenly; adding the modified composite epoxy asphalt binder to aggregates with a petroleum ratio of 8%, stirring evenly and discharging the mixture; curing at 120°C for 4 hours, and obtaining a modified composite epoxy asphalt mixture after curing.

[0054] The modified composite epoxy asphalt mixture of the present invention is prepared by using the following raw materials in weight ratio: 35-45% of high-toughness polyurethane modified epoxy resin, 1-2% of curing agent, 2-4% of compatibilizer and 50-65% of SK-70 matrix asphalt, which improves the crack resistance of the mixture and solves the problem that the epoxy resin has poor toughness and high brittleness under low temperature conditions.

[0055] See also Figure 3 , Figure 3The present invention also provides a pavement construction method for the modified composite epoxy asphalt mixture, which specifically includes the following steps:

[0056] S301: Setting the base layer by laying out the lines and leveling;

[0057] S302: Arranging a heat insulating layer on the base layer and laying a concrete base layer on the heat insulating layer;

[0058] S303: Laying epoxy asphalt waterproof bonding layer on the concrete base;

[0059] S304: Lay a modified composite epoxy asphalt mixture layer on the waterproof bonding layer.

[0060] See also Figure 4 and Figure 5 , Figure 4 The present invention is a structural cross-sectional view of a device for preparing a modified composite epoxy asphalt mixture. Figure 5 The present invention Figure 4 The present invention also provides a device for preparing the modified composite epoxy asphalt mixture, comprising a box 101, a heating plate 102, a stirrer 103, a box cover 104 and a disassembly cylinder 105;

[0061] According to this specific embodiment, the heating plate 102 is arranged at the inner bottom of the box body 101, the box cover 104 is detachably connected to the box body 101, the box cover 104 is located above the box body 101, the stirrer 103 is arranged below the box cover 104, the disassembly cylinder 105 is detachably connected to the box body 101, and the disassembly cylinder 105 is located inside the box body 101. The disassembly cylinder 105 is arranged inside the box body 101 and can be disassembled relative to the box body 101, the stirrer 103 is used to stir the mixed material inside the disassembly cylinder 105, and the heating plate 102 is used to heat the mixed material inside the disassembly cylinder 105. When preparing the modified composite epoxy asphalt mixture, firstly put the high-toughness polyurethane modified epoxy resin into the disassembly barrel 105, heat it to 100-140°C through the heating plate 102 and then take it out, then add the curing agent, compatibilizer and SK-70 matrix asphalt into the disassembly barrel 105, heat and stir it at a temperature of 100-140°C to obtain a mixture, then add the heated high-toughness polyurethane modified epoxy resin, stir it evenly to obtain the modified composite epoxy asphalt binder, then add the modified composite epoxy asphalt binder to the aggregate with a petroleum ratio of 6-8%, stir it evenly and then discharge it; maintain it at a temperature of 120-130°C for 3-4h, and obtain the modified composite epoxy asphalt mixture after curing. After preparing the modified composite epoxy asphalt mixture, the disassembly barrel 105 can be taken out from the inside of the box 101 to clean the disassembly barrel 105, thereby solving the problem of inconvenient cleaning of the inner wall of the box 101.

[0062] Secondly, a positioning bracket 106 is provided on the outside of the disassembly cylinder 105, and a positioning groove 107 adapted to the positioning bracket 106 is provided on the inside of the box 101. After the disassembly cylinder 105 and the box 101 are connected, the positioning bracket 106 is located inside the positioning groove 107. When the disassembly cylinder 105 is installed inside the box 101, the positioning bracket 106 is aligned with the positioning groove 107 and inserted to position the disassembly cylinder 105.

[0063] Specifically, the box body 101 has a discharge barrel 108, which is arranged at the outer bottom of the box body 101 and communicated with the inner side of the box body 101. The disassembly barrel 105 has a discharge port 109, and the axis of the discharge port 109 coincides with the axis of the discharge barrel 108. The discharge barrel 108 coincides with the discharge port 109, so that the prepared modified composite epoxy asphalt binder can be discharged through the discharge port 109 and the discharge barrel 108.

[0064] In addition, the device also includes a plugging cylinder, which includes a plugging column 110 and a connecting ring 111. The plugging column 110 is fixedly connected to the connecting ring 111, and the connecting ring 111 is threadedly connected to the discharge barrel 108. The plugging column 110 is located inside the discharge barrel 108. The inner side of the connecting ring 111 is provided with an internal thread, and the outer side of the discharge barrel 108 is provided with an external thread. The connecting ring 111 and the plugging column 110 are threadedly connected through the cooperation of the external thread and the internal thread, thereby realizing the disassembly between the two. The plugging column 110 blocks the inside of the discharge barrel 108 and the discharge port 109, so that when the modified composite epoxy asphalt binder is prepared, the mixed material cannot enter the discharge port 109.

[0065] What is disclosed above is only one or more preferred embodiments of the present application, and cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiments and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.

Claims

1. A device for preparing modified composite epoxy asphalt mixture, characterized in that: It comprises a box body, a heating plate, a stirrer, a box cover and a disassembly cylinder, wherein the heating plate is arranged at the inner bottom of the box body, the box cover is detachably connected to the box body, the box cover is located above the box body, the stirrer is arranged below the box cover, the disassembly cylinder is detachably connected to the box body, and the disassembly cylinder is located inside the box body; A positioning bracket is arranged on the outer side of the disassembly cylinder, and a positioning groove adapted to the positioning bracket is arranged on the inner side of the box body. After the disassembly cylinder and the box body are connected, the positioning bracket is located inside the positioning groove; The box body has a discharge barrel, which is arranged at the outer bottom of the box body and is connected to the inner side of the box body. The disassembly barrel has a discharge port, and the axis of the discharge port coincides with the axis of the discharge barrel. The device also includes a blocking cylinder, which includes a blocking column and a connecting ring. The blocking column is fixedly connected to the connecting ring, and the connecting ring is threadedly connected to the discharge cylinder. The blocking column is located inside the discharge cylinder.