A method for preparing plant powder modified chemical fiber
Through the mixed grinding and high-temperature graft copolymerization technology of negative ion powder and plant powder, the aggregation problem of plant powder is solved, the requirements of dry spinning are realized, and the modified chemical fibers are given excellent performance, including antibacterial and ultraviolet protection functions. .
Patent Information
- Application Number
- CN202311261431.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-09-27
AI Technical Summary
Hydrophilic groups in plant powders are prone to agglomeration, resulting in poor dispersion, difficult to meet the basic requirements of dry spinning of chemical fibers, and waste beneficial components in plant powders during the extraction process.
Negative ion powder is used as a friction agent and dispersant, mixed with plant powder to grind, reduce particle size and prevent agglomeration, and high-temperature grafting copolymerization and granulation are carried out in combination with polyester wax and MOFs catalyst to form stable modified chemical fibers.
It improves the dispersion and spinning performance of plant powder, achieves efficient utilization of the entire plant, retains beneficial ingredients in the plant, and imparts excellent antibacterial, ultraviolet and moisturizing properties to the modified chemical fibers.
Smart Images

Figure CN117127280B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional fibers, and in particular relates to a method for preparing plant powder-modified chemical fibers. Background Art
[0002] The content of protein, polypeptide and polysaccharide in plant powder is relatively high. During the grinding process, hydrophilic groups such as amino, hydroxyl and carboxyl groups show a large negative polarity and are easy to form agglomerates. Therefore, it is difficult to disperse plant powder in an ultrafine manner. The particle size is generally above 20μm, which is far from the basic requirements for dry spinning of chemical fibers. At present, medicinal plants such as tea that are beneficial to the human body generally use active extraction to obtain beneficial elements, and use wet spinning or microcapsule coating technology to achieve dry spinning of chemical fibers. At the same time, a large amount of beneficial components in the plant powder are wasted during the extraction process. Summary of the invention
[0003] In view of the problems in the prior art, the present invention provides a method for preparing plant powder-modified chemical fibers, which solves the problem that plant powders are very easy to agglomerate based on their own hydrophilic groups. Anion powders are used as friction agents and anion dispersants to effectively improve the dispersibility of plant powders and meet the requirements of dry spinning.
[0004] In order to achieve the above technical objectives, the technical solution of the present invention is:
[0005] A method for preparing plant powder modified chemical fiber comprises the following steps:
[0006] Step 1, mixing and grinding plant powder and negative ion powder to obtain ultrafine plant mixed powder, the main sources of the plant powder are: powder of plant leaves such as tea, bamboo leaves, mulberry leaves, rhizome powder of Chinese herbal medicines such as dendrobium, ganoderma lucidum, and Panax notoginseng; the negative ion powder adopts one or more of nano-level tourmaline, volcanic stone, jade powder, and pearl powder, the mass ratio of the plant powder to the negative ion powder is 5:4-7, the pressure of mixed grinding is 0.5-0.8Mpa, and the time of mixed grinding is 48-72h; this step utilizes the fragmentation effect of the plant powder in the mixed grinding to greatly reduce the particle size of the plant powder, and utilizes the increase in particle surface brought about by the reduction in particle size to increase the exposed amount of surface active groups, that is, in the plant powder particles The surface of the particles forms exposed active groups such as amine, hydroxyl, and carboxyl groups; the negative ion powder is a nano powder with negative ion polarity. During the mixed grinding with the plant powder, the negative ion powder is evenly dispersed in the entire mixed solid to form a uniformly dispersed system. When the negative ion powder and the plant powder both show negative ion polarity, the two form negative poles that repel each other, thereby preventing the agglomeration of the plant powder. That is, during the mixed grinding process, the negative ion powder is evenly distributed around the plant powder, and while using its own strength to break up the plant powder, it uses its own electronegativity to prevent the plant powder from agglomerating, thereby ensuring that the plant powder and the negative ion powder form a stable mixture and ultrafine; the ultrafine plant mixed powder obtained in this step meets the micron-level particle size requirement for dry spinning, that is, D90≤3μm;
[0007] Step 2, adding polyester wax to ultrafine plant mixed powder, adding MOFs catalyst and mixing evenly to obtain total ultrafine mixed powder, then high-temperature graft copolymerization and granulation of the total ultrafine mixed powder and modified chemical fiber monomer to obtain plant powder modified masterbatch, the polyester wax adopts low melting point and high temperature resistant polyester wax, and the low temperature melting point of the polyester wax is 50-60°C, and the high temperature resistant temperature is above 300°C; in the mass ratio of the total ultrafine mixed powder, the ultrafine plant mixed powder is 94%-96.5%, the polyester wax is 3%-5%, and the MOFs catalyst is 0.5%-1%; the MOFs catalyst adopts one or more of iron-based MOFs, titanium-based MOFs or zinc-based MOFs; the modified chemical The fiber monomer is one of polyamide fiber monomer, polyester fiber monomer, polyethylene fiber monomer, polypropylene fiber monomer, and polylactic acid fiber monomer; the mass ratio of the total ultrafine mixed powder to the modified chemical fiber monomer is: 15%-25% of the total ultrafine mixed powder and 75%-85% of the chemical fiber monomer powder; this step utilizes the low-temperature melting property of polyester wax to protect the plant powder, prevent high temperature from destroying the active groups in the plant powder, and form a high-temperature dispersant. At the same time, as the temperature rises, the catalytic activity of the MOFs catalyst cooperates with the electrical load system of the negative ion powder to promote the carboxyl, hydroxyl and other hydrophilic groups on the plant powder to form a stable reaction with the modified chemical fiber monomer, thereby achieving a graft copolymerization effect;
[0008] Step 3, mixing the plant powder modified masterbatch with the chemical fiber monomer slices, and dry spinning to obtain the plant powder modified chemical fiber, wherein the mass ratio of the plant powder modified masterbatch to the chemical fiber monomer slices is: 5% of the plant powder modified masterbatch and 95% of the chemical fiber monomer slices, and the chemical fiber monomer slices are one of polyamide fiber monomers, polyester fiber monomers, polyethylene fiber monomers, polypropylene fiber monomers, and polylactic acid fiber monomers.
[0009] Furthermore, the plant powder in step 1 is coarse plant powder, and its detected particle size D90 is between 20-50 μm;
[0010] Furthermore, the negative ion powder in step 1 is a nano-scale ion powder, and its detected particle size D90 is between 500-900nm;
[0011] Furthermore, the negative ion powder and the plant powder are mutually squeezed during the grinding process, and the plant powder particles are crushed by squeezing. However, in actual processing, the negative ion powder and the plant powder are both granular and have good rolling performance, which brings difficulty in mixed grinding. To solve this problem, the negative ion powder is pre-treated. The pre-treatment can not only remove impurities on the surface of the negative ion powder, reduce the impurity coverage on the surface of the negative ion powder, ensure the stability of the negative ions, and help form a negative electrode repulsive environment, but also increase the surface roughness of the negative ion powder by the pre-treatment, that is, the surface of the negative ion contains a pore structure, which greatly improves the friction of the plant powder in the negative ion powder, and can also improve the plant powder The contact between the body and the negative ion powder effectively reduces the grinding difficulty. The pretreatment method of the negative ion powder comprises the following steps: a1, placing the negative ion powder in an organic mixed solution for ultrasonic treatment for 20-30 minutes, and filtering and drying after sealed reflux reaction for 20-30 minutes to obtain clean negative ion powder; the organic mixed solution adopts an ethanol ether mixed solution, and the volume ratio of ethanol to ether is 2:4-7, the concentration of the negative ion powder in the organic mixed solution is 400-500g / L, the ultrasonic frequency of the ultrasonic treatment is 50-80kHz, and the temperature is 5-10°C; the temperature of the sealed reflux is 50-60°C, and the refluxed ether is directly introduced into the ethanol, and the drying temperature of the suction filtration and drying is 80 -90℃; this step utilizes the mutual solubility of ethanol and ether to form a homogeneous solution. When ultrasonically mixed with the negative ion powder, the organic impurities on the surface of the negative ion powder are separated, and the impurities with poor fixation on the surface are stripped off, thereby achieving a surface stripping clean treatment. During the sealed reflux process, the ether is evaporated and refluxed into the ethanol, which increases the fluidity of the ethanol and effectively improves the permeability of the organic mixed solution, thereby improving the cleaning effect; a2, the clean negative ion powder is placed in the ether for ultrasonic dispersion for 20-30 minutes, and then hydrogen chloride is introduced and a small amount of distilled water is added dropwise, and it is allowed to stand for 20-30 minutes. After ultrasonic filtration, a clean negative ion powder with a rough surface is obtained. The negative ion powder is The concentration in ether is 30-50g / L, the ultrasonic frequency of ultrasonic dispersion is 50-70kHz, and the temperature is 5-10°C; the amount of hydrogen chloride introduced is 5-10% of the mass of the negative ion powder, the amount of distilled water added is 0.01-0.05% of the volume of the ether, the standing temperature is 15-20°C, the time is 20-40min, the ultrasonic temperature of the ultrasonic filtration is 10-15°C, and the ultrasonic frequency is 70-80kHz; this step utilizes the solubility of hydrogen chloride in ether and the slight solubility of distilled water in ether to form an acid solution of a low concentration system, and utilizes the acid solution to remove inorganic impurities on the surface of the negative ion powder, and even forms certain surface corrosion, thereby improving the surface roughness of the negative ion powder.In this process, ultrasonic dispersion of ethanol and ethyl ether can remove impurities in the organic system and reduce the impact of organic impurities in the acid solution. Ether is used as the base liquid to reduce the concentration of hydrogen chloride and distilled water to form a low-acid corrosive solution, thereby cleaning and corroding the surface of the negative ion powder to obtain a negative ion powder with a clean and rough surface.
[0012] It can be seen from the above description that the present invention has the following advantages:
[0013] 1. The present invention solves the problem that plant powder is very easy to agglomerate based on its own hydrophilic groups, and uses negative ion powder as a friction agent and negative ion dispersant, which effectively improves the dispersibility of plant powder and meets the requirements of dry spinning.
[0014] 2. The plant powder of the present invention uses the plant body as raw material, realizes efficient utilization of the whole plant, and ensures the complete retention of beneficial components in the plant.
[0015] 3. Benming uses plant powder as a modifier to add a large number of amino acids and hydrophilic groups that are beneficial to the human body to the chemical fiber, which increases the moisture content of the modified chemical fiber by 8-10 times. At the same time, the skin affinity and moisturizing rate of the modified chemical fiber are effectively improved.
[0016] 4. The present invention utilizes the synergistic effect of negative ion powder and catalyst to graft copolymerize the hydrophilic groups of plant powder onto chemical fiber, and endows the modified chemical fiber with excellent antibacterial properties, as well as negative ion / ultraviolet protection / far infrared and other functions. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is an electron microscope comparison of the coarse tea powder and the ultrafine mixed powder in Example 1;
[0018] Figure 2 The filtration value test of PA masterbatch modified with tea powder in Example 1;
[0019] Figure 3 The filtration value test of the tea powder modified PBT masterbatch in Example 2;
[0020] Figure 4 This is the filtration value test of the Ganoderma lucidum powder modified polylactic acid masterbatch in Example 3. DETAILED DESCRIPTION
[0021] Combination Figures 1 to 4 , describes in detail the specific embodiments of the present invention, but does not limit the claims of the present invention.
[0022] Example 1
[0023] A method for preparing plant powder modified chemical fiber
[0024] Step 1, the negative ion powder is a mixture of tourmaline and pearl powder, and the mass ratio of the two is 70% tourmaline and 30% pearl powder, and the detected particle size D90 is between 500-900nm. The pretreatment method of the negative ion powder includes the following steps: a1, placing the negative ion powder in an organic mixed solution for ultrasonic treatment for 20 minutes, filtering and drying after sealed reflux reaction for 20 minutes to obtain clean negative ion powder; the organic mixed solution is an ethanol ether mixed solution, and the volume ratio of ethanol to ether is 2:4, the concentration of the negative ion powder in the organic mixed solution is 400g / L, the ultrasonic frequency of the ultrasonic treatment is 50kHz, and the temperature is 5°C; the temperature of the sealed reflux is 50°C , and the refluxed ether is directly introduced into the ethanol, and the drying temperature of the suction filtration and drying is 80°C; a2, the clean negative ion powder is placed in the ether for ultrasonic dispersion for 20 minutes, and then hydrogen chloride is introduced and a small amount of distilled water is added dropwise, and the mixture is allowed to stand for 20 minutes. After ultrasonic filtration, a clean negative ion powder with a rough surface is obtained, and the concentration of the negative ion powder in the ether is 30g / L, the ultrasonic frequency of the ultrasonic dispersion is 50kHz, and the temperature is 5°C; the amount of hydrogen chloride introduced is 5% of the mass of the negative ion powder, the amount of distilled water added is 0.01% of the volume of the ether, the standing temperature is 15°C, the time is 20 minutes, the ultrasonic temperature of the ultrasonic filtration is 10°C, and the ultrasonic frequency is 70kHz;
[0025] Step 2, mixing and grinding the plant powder and the negative ion powder to obtain ultrafine plant mixed powder, wherein the plant powder is tea powder, and its particle size D90 is between 20-50 μm; the mass ratio of the plant powder to the negative ion powder is 1:1, the mixed grinding pressure is 0.7 MPa, and the mixed grinding time is 50 hours; the plant powder; after particle size detection, the ultrafine plant mixed powder has D90: 2.2 microns, D50: 1.2 microns, and has met the ultrafine spinning conditions; Figure 1 As shown in the figure, the powder after mixing and grinding has good dispersibility.
[0026] Step 3, adding polyester wax to the ultrafine plant mixed powder, and adding MOFs catalyst to mix evenly to obtain a total ultrafine mixed powder, and then the total ultrafine mixed powder and the modified chemical fiber monomer are subjected to high-temperature graft copolymerization granulation to obtain a plant powder modified masterbatch, wherein the polyester wax adopts Euroceras 691 polyester wax; the mass ratio of the total ultrafine mixed powder is 94% ultrafine plant mixed powder, 5% polyester wax, and 1% MOFs catalyst; the MOFs catalyst adopts iron-based MOF; the modified chemical fiber monomer adopts PA monomer; the mass ratio of the total ultrafine mixed powder to the modified chemical fiber monomer is: 22% total ultrafine mixed powder, 78% chemical fiber monomer powder; Figure 2The filtration value graph shown in the figure shows that the filterability of PA masterbatch is very good through the filtration value detection and analysis, which is suitable for spinning requirements; the filtration value graph also shows that under the high temperature protection and catalytic action of polyester wax, the protein polypeptides and polysaccharide components in the tea powder do not form agglomeration and agglomeration, and a graft copolymerization reaction occurs, so that the dispersion fluidity is good and the spinning filtration performance meets the standard;
[0027] Step 4, mixing the plant powder modified masterbatch with the chemical fiber monomer slices, and dry spinning to obtain the plant powder modified nylon filament, the mass ratio of the plant powder modified masterbatch to the chemical fiber monomer slices is: 5% of the plant powder modified masterbatch and 95% of the chemical fiber monomer slices, and the chemical fiber monomer slices use polyamide fiber monomers; the temperature of the dry spinning is 220-260°C.
[0028] Comparative analysis of the polyester filament prepared in this example and tea leaves shows that the protein polypeptides, starch and cellulose in tea leaves are effectively protected during high-temperature granulation and spinning. The specific data are as follows:
[0029]
[0030]
[0031] The amino acid content is slightly higher after conversion, which is related to the amino acids contained in the pearl powder in the mixed powder, and there is almost no loss of starch and cellulose. Among them, the amino acid content test of the above products adopts standard FZ / T50049-2020, the cellulose content test adopts the anthrone-sulfuric acid colorimetric method; the starch content test adopts the anthrone sulfate method.
[0032] The tea-modified polyamide fiber of Example 1 was tested for moisture content and antistatic resistivity compared with ordinary polyamide fiber. The data are as follows, which show that the modification method provided in the present application has a good effect.
[0033] Among them, the evaluation of the resistivity of this product adopts the national standard GB / T 12703.4-2010.
[0034] Moisture content Specific resistance Polyamide fiber 0.68% <![CDATA[8.2X10 11 ]]> Tea leaves modified polyamide fiber 6.12% <![CDATA[5.8X10 8 ]]>
[0035] Example 2
[0036] A method for preparing plant powder modified chemical fiber
[0037] Step 1, the negative ion powder is a mixture of tourmaline and pearl powder, and the mass ratio of the two is 70% tourmaline and 30% pearl powder, and the detected particle size D90 is between 500-900nm. The pretreatment method of the negative ion powder includes the following steps: a1, placing the negative ion powder in an organic mixed solution for ultrasonic treatment for 30 minutes, and filtering and drying after sealed reflux reaction for 30 minutes to obtain clean negative ion powder; the organic mixed solution is an ethanol ether mixed solution, and the volume ratio of ethanol to ether is 2:7, the concentration of the negative ion powder in the organic mixed solution is 500g / L, the ultrasonic frequency of the ultrasonic treatment is 80kHz, and the temperature is 10°C; the temperature of the sealed reflux is 60°C, The refluxed ether is directly introduced into the ethanol, and the drying temperature of the suction filtration and drying is 90°C; a2, the clean negative ion powder is ultrasonically dispersed in the ether for 30 minutes, and then hydrogen chloride is introduced and a small amount of distilled water is added dropwise, and the mixture is allowed to stand for 30 minutes. After ultrasonic filtration, a clean negative ion powder with a rough surface is obtained, wherein the concentration of the negative ion powder in the ether is 50g / L, the ultrasonic frequency of the ultrasonic dispersion is 70kHz, and the temperature is 10°C; the amount of hydrogen chloride introduced is 10% of the mass of the negative ion powder, the amount of distilled water added is 0.05% of the volume of the ether, the standing temperature is 20°C, the time is 40 minutes, the ultrasonic temperature of the ultrasonic filtration is 15°C, and the ultrasonic frequency is 80kHz;
[0038] Step 2, mixing and grinding the plant powder and the negative ion powder until D90≤3 microns to obtain ultrafine plant mixed powder, wherein the plant powder is tea powder, and its particle size D90 is between 20-50 μm; the mass ratio of the plant powder to the negative ion powder is 1:1, the mixed grinding pressure is 0.8 Mpa, and the mixed grinding time is 60 hours;
[0039] Step 3, adding polyester wax to the ultrafine plant mixed powder, and adding MOFs catalyst to mix evenly to obtain a total ultrafine mixed powder, and then the total ultrafine mixed powder and the modified chemical fiber monomer are subjected to high-temperature graft copolymerization granulation to obtain a plant powder modified masterbatch, wherein the polyester wax adopts Euroceras 694 polyester wax; the mass ratio of the total ultrafine mixed powder is 96.5% of ultrafine plant mixed powder, 3% of polyester wax, and 0.5% of MOFs catalyst; the MOFs catalyst adopts titanium-based MOFs; the modified chemical fiber monomer adopts PBT monomer; the mass ratio of the total ultrafine mixed powder to the modified chemical fiber monomer is: 18% of the total ultrafine mixed powder and 82% of the chemical fiber monomer powder; Figure 3The filtration value graph shown in the figure shows that the filtration performance of PBT masterbatch is very good and suitable for spinning requirements through filtration value detection and analysis. The filtration value graph also shows that under the high temperature protection and catalytic action of polyester wax, the protein polypeptides and polysaccharide components in the tea powder do not form agglomeration and agglomeration, and a graft copolymerization reaction occurs, so that the dispersion fluidity is good and the spinning filtration performance meets the standard.
[0040] Step 4, mixing the plant powder modified masterbatch with the chemical fiber monomer slices, and dry spinning to obtain the plant powder modified polyester fiber filaments, wherein the mass ratio of the plant powder modified masterbatch to the chemical fiber monomer slices is: 5% of the plant powder modified masterbatch and 95% of the chemical fiber monomer slices, and the chemical fiber monomer slices use polyester fiber monomers; the temperature of the dry spinning is 270-290°C.
[0041] Comparative analysis of the polyester fiber filaments prepared in this example and tea leaves shows that the protein polypeptides, starch and cellulose in tea leaves are effectively protected during high-temperature granulation and spinning. The specific data are as follows:
[0042]
[0043] After conversion, the amino acid content is slightly higher, which is related to the amino acids contained in the pearl powder in the mixed powder, and there is almost no loss of starch and cellulose.
[0044] The tea-modified polyester fiber of Example 2 was tested for moisture content and antistatic resistivity compared with ordinary polyester fiber. The data are as follows, which show that the modification method provided in the present application has a good effect.
[0045]
[0046]
[0047] Example 3
[0048] A method for preparing plant powder modified chemical fiber
[0049] Step 1, the negative ion powder is a mixture of volcanic rock and jade powder, and the mass ratio of the two is 70% volcanic rock powder and 30% jade powder, and the detected particle size D90 is between 500-900nm. The pretreatment method of the negative ion powder includes the following steps: a1, placing the negative ion powder in an organic mixed solution for ultrasonic treatment for 25 minutes, filtering and drying after sealed reflux reaction for 25 minutes to obtain clean negative ion powder; the organic mixed solution is an ethanol ether mixed solution, and the volume ratio of ethanol to ether is 2:5, the concentration of the negative ion powder in the organic mixed solution is 450g / L, the ultrasonic frequency of the ultrasonic treatment is 70kHz, and the temperature is 8°C; the temperature of the sealed reflux is 50°C , and the refluxed ether is directly introduced into the ethanol, and the drying temperature of the suction filtration and drying is 85°C; a2, the clean negative ion powder is placed in the ether for ultrasonic dispersion for 25 minutes, and then hydrogen chloride is introduced and a small amount of distilled water is added dropwise, and the mixture is allowed to stand for 25 minutes. After ultrasonic filtration, a clean negative ion powder with a rough surface is obtained, the concentration of the negative ion powder in the ether is 40g / L, the ultrasonic frequency of the ultrasonic dispersion is 60kHz, and the temperature is 8°C; the amount of hydrogen chloride introduced is 8% of the mass of the negative ion powder, the amount of distilled water added is 0.03% of the volume of the ether, the standing temperature is 18°C, the time is 30 minutes, the ultrasonic temperature of the ultrasonic filtration is 12°C, and the ultrasonic frequency is 75kHz;
[0050] Step 2, mixing and grinding the plant powder and the negative ion powder until D90≤3 microns to obtain ultrafine plant mixed powder, wherein the plant powder is coarse Ganoderma lucidum powder, and its particle size D90 is between 20-50 μm; the mass ratio of the plant powder to the negative ion powder is 1:1, the pressure of the mixed grinding is 0.8 Mpa, and the time of the mixed grinding is 60 hours;
[0051] Step 3, adding polyester wax to the ultrafine plant mixed powder, and adding MOFs catalyst to mix evenly to obtain a total ultrafine mixed powder, and then the total ultrafine mixed powder and the modified chemical fiber monomer are subjected to high-temperature graft copolymerization granulation to obtain a plant powder modified masterbatch, wherein the polyester wax adopts Euroceras 691 polyester wax; the mass ratio of the total ultrafine mixed powder is 95.2% of ultrafine plant mixed powder, 4% of polyester wax, and 0.8% of MOFs catalyst; the MOFs catalyst adopts titanium-based MOFs; the modified chemical fiber monomer adopts polylactic acid monomer; the mass ratio of the total ultrafine mixed powder to the modified chemical fiber monomer is: 20% of the total ultrafine mixed powder and 80% of the chemical fiber monomer powder; Figure 4The filtration value graph shown in the figure shows that the filterability of polylactic acid masterbatch is very good and suitable for spinning requirements through filtration value detection and analysis. The filtration value graph also shows that under the high temperature protection and catalytic action of polyester wax, the protein polypeptides and polysaccharide components in the tea powder do not form agglomeration and agglomeration, and a graft copolymerization reaction occurs, so that the dispersion fluidity is good and the spinning filtration performance meets the standard.
[0052] Step 4, mixing the plant powder modified masterbatch with the chemical fiber monomer slices, and dry spinning to obtain the plant powder modified polylactic acid fiber filaments, wherein the mass ratio of the plant powder modified masterbatch to the chemical fiber monomer slices is: 5% of the plant powder modified masterbatch and 95% of the chemical fiber monomer slices, and the chemical fiber monomer slices use polylactic acid monomers; the temperature of the dry spinning is 230-250°C.
[0053] Comparative analysis of the polylactic acid fiber filaments prepared in this example and the ganoderma lucidum powder shows that the protein polypeptides, starch and cellulose in the tea leaves are effectively protected during high-temperature granulation and spinning. The specific data are as follows:
[0054]
[0055] The moisture content and antistatic resistivity of the ganoderma-modified polylactic acid fiber of Example 3 were compared with those of ordinary polylactic acid fibers, and the data are as follows, which show that the modification method provided in the present application has a good effect.
[0056] Moisture content Specific resistance Polylactic acid fiber 0.02% <![CDATA[6.9X10 12 ]]> Ganoderma lucidum modified polylactic acid fiber 2.35% <![CDATA[3.6X10 9 ]]>
[0057] Through the tests of Examples 1-3, it can be concluded that the water content of the plant powder modified chemical fiber provided by the present application is increased by 8-10 times, its skin-friendly and moisturizing effect is well improved, and the antistatic effect is also improved to a certain extent. And from the appearance of the plant powder modified chemical fiber, the modified chemical fiber is obviously fluffy and soft, with the silky feeling of amino acids and hydrophilic groups.
[0058] The modified chemical fibers of Examples 1-3 contain nano-anion powder and metal-based catalyst powder to ensure that the modified chemical fibers and their fabrics have good antibacterial properties, anion properties, UV protection and far infrared properties. The performance tests are as follows:
[0059]
[0060]
[0061] Among them, the evaluation of the antibacterial performance of this product adopts the national standard GB / T 20944.1-2008.
[0062] The fibers of Examples 1-3 were made into fabrics, and performance tests were performed based on the fabrics, wherein:
[0063] A: Tea modified polyamide fabric, weight 160g / m2; 92% tea modified polyamide fiber; 8% spandex
[0064] B: Tea modified polyester fabric, weight 160g / m2; 92% tea modified polyester fiber; 8% spandex
[0065] C: Ganoderma lucidum modified polylactic acid fabric, weight 160g / m2; 92% Ganoderma lucidum modified polylactic acid fiber; 8% spandex
[0066] Negative ions (pcs / cm3) UV protection Far infrared emissivity A 920 >UPF50+ 0.89 B 850 >UPF50+ 0.90 C 760 >UPF50+ 0.91
[0067] The test shows that the fabric prepared by the fiber of the technical solution has good antibacterial performance, negative ion performance, UV protection and far infrared performance. Among them, the above-mentioned negative ion detection adopts the national standard GB / T30128-2013; the evaluation of UV protection adopts the national standard GB / T18830-2009; the evaluation of far infrared emissivity adopts the national standard GB / T 30127-2013.
[0068] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A method for preparing plant powder modified chemical fiber, characterized in that: The steps include: Step 1, mixing and grinding the plant powder and the negative ion powder to obtain ultrafine plant mixed powder; Step 2, adding polyester wax to the ultrafine plant mixed powder, and adding MOFs catalyst to mix evenly to obtain a total ultrafine mixed powder, and then high-temperature graft copolymerization and granulation of the total ultrafine mixed powder and modified chemical fiber to obtain a plant powder modified masterbatch; Step 3, mixing the plant powder modified masterbatch with the chemical fiber slices, and dry spinning to obtain the plant powder modified chemical fiber; The modified chemical fiber in step 2 is one of polyamide fiber, polyester fiber and polylactic acid fiber; the mass ratio of the total ultrafine mixed powder to the modified chemical fiber is: 15%-25% of the total ultrafine mixed powder and 75-85% of the modified chemical fiber powder; The mass ratio of the plant powder modified masterbatch to the chemical fiber slices in step 3 is: 5% of the plant powder modified masterbatch and 95% of the chemical fiber slices, and the chemical fiber slices are made of one of polyamide fiber, polyester fiber and polylactic acid fiber.
2. The method for preparing plant powder-modified chemical fiber according to claim 1, characterized in that: The plant powder in step 1 is coarse plant powder, and its detected particle size D90 is between 20-50 μm.
3. The method for preparing plant powder-modified chemical fiber according to claim 1, characterized in that: The negative ion powder in step 1 is a nano-sized negative ion powder, and its detected particle size D90 is between 500-900nm.
4. The method for preparing plant powder-modified chemical fiber according to claim 3, characterized in that: The main sources of the plant powder in step 1 are: powder of tea leaves, bamboo leaves, mulberry leaves, and rhizome powder of dendrobium, ganoderma lucidum, and Panax notoginseng; the nano-level negative ion powder is one or more of nano-level tourmaline, volcanic stone, jade powder, and pearl powder.
5. The method for preparing plant powder-modified chemical fiber according to claim 1, characterized in that: The mass ratio of the plant powder to the negative ion powder in step 1 is 5:4-7, the pressure of the mixed grinding is 0.5-0.8 MPa, and the time of the mixed grinding is 48-72 hours.
6. The method for preparing plant powder-modified chemical fiber according to claim 1, characterized in that: The polyester wax in step 2 is a low-melting-point, high-temperature-resistant polyester wax, and the low-temperature melting point of the polyester wax is 50-60°C, and the high-temperature-resistant temperature is above 300°C; the mass ratio of the total ultrafine mixed powder is 94%-96.5% of the ultrafine plant mixed powder, 3%-5% of the polyester wax, and 0.5%-1% of the MOFs catalyst.
7. The method for preparing plant powder-modified chemical fiber according to claim 1, characterized in that: The MOFs catalyst in step 2 is one or more of iron-based MOFs, titanium-based MOFs or zinc-based MOFs.