A safer root canal file
By forming a titanium nitride layer on the root canal file, the problem of Ni ion dissolution in the nickel-titanium root canal file is solved, its safety and corrosion resistance are improved, the processing technology is simplified, and the Ni ion seepage is prevented. Effective obstruction.
Patent Information
- Application Number
- CN202311192502.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-09-15
AI Technical Summary
The dissolution of Ni ions in existing nickel-titanium root canal files can cause toxic side effects such as sensitization and teratogenesis to the human body. The method for preventing Ni ion dissolution in existing nickel-titanium alloy root canal files is complex and insufficiently safe.
Vacuum isothermal nitriding technology is used to form a uniform and dense titanium nitride layer on the surface of the root canal file base. Through high-temperature treatment and repeated stretching/unloading operations in a specific gas environment, a titanium nitride coating with excellent corrosion resistance is formed. layer.
It effectively blocks the infiltration of Ni ions, reduces the amount of nickel ion dissolution, improves the safety and corrosion resistance of root canal files, while maintaining the original properties of the shape memory alloy and simplifying the processing technology.
Smart Images

Figure CN117137651B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of biomedical metal products, and in particular to a root canal file with better safety. Background Art
[0002] Pulp disease and periapical periodontitis are common oral diseases, and root canal therapy is the main treatment for them. Root canal preparation is one of the key factors that determine the success or failure of root canal treatment, and the effect of root canal preparation is largely related to the appropriate root canal preparation instruments. However, clinical studies have shown that the Ni ions contained in Ni-Ti alloys of nickel-titanium root canal preparation instruments are a potential allergenic factor, and the dissolution of Ni ions can cause toxic and side effects such as allergy and teratogenicity to the human body.
[0003] In view of the above situation, preparing a surface coating on a nickel-titanium alloy root canal file material is an effective means to prevent Ni ion dissolution. For example, Chinese patent application CN116356257A discloses a process method for a nickel-titanium alloy root canal file and a nickel-titanium alloy root canal file, comprising: cleaning the nickel-titanium alloy root canal file; forming a nano coating on the outer surface of the root canal file, wherein the nano coating is a Ni-La composite coating.
[0004] At present, there is still an urgent need for a root canal file with a titanium nitride layer that has a simpler preparation method, higher safety and practicality.
[0005] The information in the background technology is only for illustrating the general background of the present invention and should not be regarded as admitting or suggesting in any form that such information constitutes the prior art known to a person skilled in the art. Summary of the invention
[0006] In order to solve at least some of the technical problems in the prior art, the present invention provides a root canal file having a titanium nitride layer and a use thereof. Specifically, the present invention includes the following contents.
[0007] A first aspect of the present invention provides a safer root canal file with a titanium nitride layer, comprising a root canal file base and a titanium nitride layer located on the surface of the root canal file base, wherein the titanium nitride layer is golden in surface and is uniformly and densely coated on the root canal file base.
[0008] In certain embodiments, according to the root canal file with better safety of the present invention, the root canal file having a titanium nitride layer has a good titanium nitride layer and no cracks under a fatigue test condition of 90 degree fatigue 1500 times.
[0009] In certain embodiments, according to the root canal file with better safety according to the present invention, the presence of the titanium nitride layer makes the nickel ion dissolution amount of the root canal file having the titanium nitride layer lower than 0.025 μg / L in 10 days.
[0010] In certain embodiments, according to the root canal file with better safety according to the present invention, the molar ratio of titanium metal to nickel metal in the root canal file base is 50:50 to 55:45.
[0011] In certain embodiments, the root canal file with better safety according to the present invention is obtained by forming a titanium nitride layer on the surface of the base body through vacuum isothermal nitriding technology.
[0012] In certain embodiments, the root canal file with better safety according to the present invention is prepared by the following steps:
[0013] a. Smelting titanium metal and nickel metal under non-oxidizing conditions, then heating to 1200-1400°C under inert gas protection or vacuum environment, respectively performing high temperature refining, and then cooling to 600-1000°C for casting to obtain nickel-titanium memory alloy, and processing to obtain wire;
[0014] b. The wire is processed by a root canal file, and the root canal file substrate of the required specifications is ground, and kept in a nitrogen mixed gas environment with a gas pressure of 0.005 to 0.1Mpa and a temperature of 550-600°C for 0.5-5 hours. After cooling, it is kept in an argon environment at 500-550°C for 0.5-5 hours, and then furnace cooled.
[0015] In certain embodiments, the root canal file with better safety according to the present invention further comprises the step of strengthening the nickel-titanium memory alloy or the processed root canal file, wherein the strengthening treatment refers to the step of repeatedly stretching / unloading the nickel-titanium memory alloy or the processed root canal file and performing high temperature treatment in an inert environment.
[0016] In certain embodiments, according to the root canal file with better safety according to the present invention, the stretching deformation is 1-6%, which is repeated 5-20 times.
[0017] In certain embodiments, according to the root canal file with better safety described in the present invention, the obtained wire is processed by a root canal file processing grinder to grind out a root canal file base of the required specifications, and is kept in a nitrogen-containing mixed gas environment with a gas pressure of 0.005 to 0.1 MPa and a temperature of 550-600° C. for 0.5-5 hours, and after cooling, is kept in an argon gas environment of 500-550° C. for 0.5-5 hours, and then furnace-cooled; the root canal file is subjected to repeated stretching / unloading operations, and then, is heat-treated in an inert environment of 300-550° C. for 1-10 hours; or the obtained wire is subjected to Repeat the stretching deformation and unloading operations, and then keep it warm in an inert gas environment at 300-550°C; pass the treated wire through a root canal file processing grinder to grind out a root canal file base of the required specifications, keep it in a nitrogen-containing mixed gas environment with a gas pressure of 0.005 to 0.1 MPa and a temperature of 550-600°C for 0.5-5 hours, and after cooling, keep it in an argon gas environment at 500-550°C for 0.5-5 hours, and then furnace cool; repeat the stretching / unloading operations on the root canal file, and then keep it warm in an inert environment at 300-550°C for 1-10 hours.
[0018] In certain embodiments, according to the root canal file with better safety according to the present invention, the nitrogen-containing mixed gas includes nitrogen and argon.
[0019] In certain embodiments, according to the root canal file with better safety according to the present invention, the volume ratio of nitrogen gas to argon gas is 0.8:1 to 1:0.8.
[0020] In certain embodiments, according to the root canal file with better safety according to the present invention, the cumulative amount of wire processing is controlled to be 17-60%.
[0021] The second aspect of the present invention provides a method for preparing the root canal file having a titanium nitride layer according to the present invention.
[0022] The root canal file with a titanium nitride layer of the present invention has better safety and practicality. The NiTi shape memory alloy root canal file with a titanium nitride layer prepared by heat treatment nitriding technology has excellent corrosion resistance and can prevent Ni ion leakage during use to reduce toxic effects on the human body. In addition, the processing and heat treatment methods used in the present invention are simple in process, but have excellent corrosion resistance while maintaining the original performance of the shape memory alloy, thereby achieving excellent protection capabilities. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a surface image of the root canal file obtained in Example 1;
[0024] Figure 2This is the surface image of the root canal file obtained in Comparative Example 2. The root canal file is locally oxidized and appears earthy yellow, dark purple or blue, indicating that the original nitride layer is destroyed in the environment of high temperature insulation and without argon protection. DETAILED DESCRIPTION
[0025] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0026] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that the upper and lower limits of the scope and each intermediate value therebetween are specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0027] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art to which the invention belongs. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0028] Safer root canal files
[0029] A first aspect of the present invention provides a root canal file with better safety, comprising a root canal file base and a titanium nitride layer located on the surface of the root canal file base, wherein the titanium nitride layer is golden yellow in surface and is evenly and densely coated on the root canal file base.
[0030] The titanium nitride layer of the root canal file of the present invention has excellent stability. On the one hand, it is not easily oxidized, so that its surface presents a uniform golden yellow color. The existing coating or protective layer is easy to present different colors due to oxidation, such as partial or even the entire surface presenting khaki, dark purple or blue. On the other hand, the titanium nitride layer of the present invention has excellent fatigue resistance, and no obvious cracks will appear even after 1000 times or even 1500 times of fatigue at 90 degrees.
[0031] In the present invention, due to the presence of the titanium nitride layer, the nickel ion dissolution amount of the root canal file having the titanium nitride layer is lower than 0.025 μg / L, especially lower than 0.020 μg / L, for example lower than 0.010 μg / L, or even lower than 0.005 μg / L in 10 days. In another embodiment, due to the presence of the titanium nitride layer, the nickel ion dissolution amount of the root canal file having the titanium nitride layer is lower than 0.4 μg / L, especially lower than 0.3 μg / L, for example lower than 0.2 μg / L, or even lower than 0.1 μg / L in 1 day.
[0032] In the present invention, the molar ratio of titanium metal to nickel metal in the root canal file base is 50:50-55:45, preferably 51-54:46-48.
[0033] Preparation method
[0034] The present invention also provides a method for preparing a root canal file having a titanium nitride layer, which comprises at least the following steps: (1) a wire preparation step, (2) a titanium nitride layer step, and (3) an optional strengthening step. Those skilled in the art should understand that the numbers (1), (2) and (3) are only for the purpose of distinguishing different steps, and do not mean the order of the steps. As long as the purpose of the present invention can be achieved, the order of the above steps is not particularly limited. In addition, those skilled in the art should also understand that other steps or operations may be included before or after the above steps (1)-(3), or between these arbitrary steps, such as further optimizing and / or improving the method of the present invention. Each step is described in detail below.
[0035] Steps for preparing wire:
[0036] The wire preparation steps of the present invention include smelting titanium metal and nickel metal under the condition of ensuring that titanium is not oxidized, then, under the protection of inert gas or vacuum environment, raising the initial temperature to 1200-1400°C, performing high-temperature refining respectively, standing and then cooling to 600-1000°C for casting to obtain nickel-titanium memory alloy, and processing to obtain wire.
[0037] In the present invention, the inert atmosphere environment is included under non-oxidizing conditions. The smelting can be carried out in a crucible, for example. In the preparation method of the present invention, the amount of titanium metal and nickel metal used as raw materials is generally based on the molar ratio, and titanium metal is basically slightly higher than nickel metal. For example, the molar ratio of titanium metal to nickel metal is 50:50 to 55:45. Within the above range, it is easy to obtain the effect of maintaining the shape memory function while facilitating the nitriding reaction. If the proportion of titanium metal is too high, the shape memory function is affected. On the other hand, if the proportion of nickel metal is too high, nickel is more likely to precipitate.
[0038] In the present invention, the temperature during refining is generally 1200-1400°C, such as 1250°C, 1300°C, 1350°C, etc. There is no particular limitation on this. After refining, the temperature is lowered for pouring, and the temperature during pouring is generally lowered to 600-1000°C, such as 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, etc.
[0039] Titanium nitride layer preparation steps:
[0040] The titanium nitride layer preparation steps of the present invention include processing the obtained wire material with a root canal file, grinding a root canal file substrate of required specifications, keeping it in a nitrogen-containing mixed gas environment with a gas pressure of 0.005 to 0.1 MPa and a temperature of 550-600° C. for 0.5-5 hours, cooling it, keeping it in an argon gas environment of 500-550° C. for 0.5-5 hours, and then furnace cooling it.
[0041] In the present invention, the wire is processed and / or ground to obtain the root canal file base. The size of the root canal file base is not limited and can be adjusted as needed. The processing can use known processing tools.
[0042] In the present invention, the nitriding step includes subjecting the root canal file substrate to a vacuum isothermal nitriding treatment in a low-pressure nitrogen-containing mixed gas, and maintaining the time sufficient to form a continuous nitrided layer on the surface, for example, 0.5-5 hours, preferably 1-4 hours, such as 2 hours, 3 hours. The volume ratio of nitrogen and argon in the mixed gas is not particularly limited, and is generally 0.8:1 to 1:0.8. Within this range, the generation rate or penetration effect of titanium nitride can be advantageously controlled. If the nitrogen ratio is too high, although the penetration rate is increased, the bonding strength tends to decrease, which is also not conducive to obtaining excellent fatigue resistance of the titanium nitride coating. On the other hand, if the nitrogen ratio is too low, it is not conducive to forming an effective titanium nitride coating thickness.
[0043] The present invention has found that although the titanium nitride layer obtained after the above-mentioned nitriding treatment has good integrity, it is easily oxidized. The inventors further studied and found that further adding an argon high-temperature treatment step after the nitriding treatment can effectively prevent the obtained titanium nitride from being oxidized. The anti-oxidation treatment includes keeping the obtained titanium nitride layer in a high-temperature argon environment for 0.5-5 hours after cooling, and then furnace cooling to room temperature. The temperature of the anti-oxidation treatment is generally lower than the temperature during the nitriding treatment, usually 500-550°C, such as 510°C, 520°C, 540°C, 550°C.
[0044] Strengthening steps
[0045] The strengthening step of the present invention comprises subjecting the nickel-titanium memory alloy or the processed root canal file to repeated stretching / unloading operations and high-temperature treatment in an inert environment.
[0046] In the present invention, the stretching generally causes the deformation to be 1-6%, such as 2%, 3%, 4%, 5%, etc. After stretching, unloading is required, that is, the tensile stress is removed and the material recovers automatically. Stretching and unloading are repeated for multiple times, for example, 5-20 times, such as 6 times, 8 times, 10 times, 12 times, 14 times, 16 times and 18 times.
[0047] In the present invention, after the repeated stretching and unloading operations, heat treatment is further included in a high-temperature inert environment. At this time, the high temperature is generally 300-550°C, such as 350°C, 400°C, 450°C, 500°C, etc. The heat treatment time is generally 1-10 hours, preferably more than 5 hours, such as 6 hours, 7 hours, 8 hours, etc. The inert environment includes an inert gas environment, such as argon, helium, etc.
[0048] Example 1
[0049] This embodiment exemplifies a method for preparing a root canal file having a surface protective titanium nitride layer, comprising the following steps:
[0050] 1. Preparation of nickel-titanium shape memory alloy
[0051] A CaO crucible with high temperature stability is selected for smelting, and the composition of Ni and Ti is accurate by ensuring that Ti is not oxidized to avoid Ti forming oxides that cause changes in the composition ratio, and a shape memory alloy with a stable NiTi phase transition temperature is obtained. Among them, the molar ratio of titanium metal to nickel metal is 52:48.
[0052] Under inert gas protection and vacuum degree guaranteed to be 10 -2 In a support environment, the initial temperature is first raised to 1200°C, high-temperature refining is performed for 5 minutes, and then the temperature is lowered to 800°C for pouring after standing for 5 minutes. After the nickel-titanium memory alloy is obtained by pouring, it is processed to obtain the required wire material, and the cumulative processing amount is 30%.
[0053] 2. Preparation of surface protective titanium nitride layer
[0054] The nickel-titanium shape memory alloy wire obtained in step 1 is passed through a root canal file processing grinder to grind out a root canal file substrate of the required specifications. The processed root canal file substrate is heat-treated to obtain a root canal file with a surface protective coating. The heat treatment includes: in a nitrogen and argon mixed environment with a gas pressure of 0.05MPa, the insulation temperature is 550°C, and the insulation time is 1h. After cooling, in an argon environment with a gas pressure of 0.05MPa, the insulation temperature is 500°C, the insulation time is 1h, and the furnace is cooled for more than 4h to prepare the coating.
[0055] Example 2
[0056] This embodiment exemplifies a method for preparing a root canal file having a surface protective titanium nitride layer, comprising the following steps:
[0057] 1. Preparation of nickel-titanium shape memory alloy
[0058] A CaO crucible with high temperature stability is selected for smelting, and the composition of Ni and Ti is accurate by ensuring that Ti is not oxidized to avoid Ti forming oxides that cause changes in the composition ratio, and a shape memory alloy with a stable NiTi phase transition temperature is obtained. Among them, the molar ratio of titanium metal to nickel metal is 52:48.
[0059] Under inert gas protection and vacuum degree guaranteed to be 10 -2 In a support environment, the initial temperature is first raised to 1200°C, high-temperature refining is performed for 5 minutes, and then the temperature is lowered to 800°C for pouring after standing for 5 minutes. After the nickel-titanium memory alloy is obtained by pouring, it is processed to obtain the required wire material, and the cumulative processing amount is 30%.
[0060] 2. Preparation of surface protective titanium nitride layer
[0061] The nickel-titanium shape memory alloy wire obtained in step 1 is passed through a root canal file processing grinder to grind out a root canal file substrate of the required specifications. The processed root canal file substrate is heat-treated to obtain a root canal file with a surface protective coating. The heat treatment includes: in a nitrogen and argon mixed environment with a gas pressure of 0.05MPa, the insulation temperature is 550°C, and the insulation time is 1h. After cooling, in an argon environment with a gas pressure of 0.05MPa, the insulation temperature is 500°C, the insulation time is 1h, and the furnace is cooled for more than 4h to prepare the coating.
[0062] 3. Strengthening treatment
[0063] The root canal file was stretched to 5% at room temperature and then unloaded, and this operation was repeated 10 times. Next, it was heat-treated in an inert gas environment at 400° C. for 8 hours.
[0064] Example 3
[0065] This embodiment is a method for preparing a root canal file that is first strengthened and then nitrided, comprising the following steps:
[0066] 1. Preparation of nickel-titanium shape memory alloy:
[0067] A CaO crucible with high temperature stability is selected for smelting, and the composition of Ni and Ti is accurate by ensuring that Ti is not oxidized to avoid Ti forming oxides that cause changes in the composition ratio, and a shape memory alloy with a stable NiTi phase transition temperature is obtained. Among them, the molar ratio of titanium metal to nickel metal is 52:48.
[0068] Use inert gas protection and vacuum degree guaranteed to be 10 -2In a support environment, the initial temperature is first raised to 1200°C, high-temperature refining is performed for 5 minutes, and then the temperature is lowered to 800°C for pouring after standing for 5 minutes. After the nickel-titanium memory alloy is cast, it is processed to obtain the required wire material, and the cumulative processing amount is 30%.
[0069] 2. Strengthening treatment
[0070] The obtained wire material was stretched to 5% at room temperature and then unloaded, and this operation was repeated 8 times. Next, it was heat-treated in an inert gas environment at 400°C for 8 hours.
[0071] 3. Preparation of surface protective titanium nitride layer
[0072] The nickel-titanium shape memory alloy wire obtained in step 2 is passed through a root canal file processing grinder to grind out a root canal file substrate of the required specifications. The processed root canal file substrate is heat-treated to obtain a root canal file with a surface protective coating. The heat treatment includes: in a nitrogen and argon mixed environment with a gas pressure of 0.05MPa, the insulation temperature is 550°C, and the insulation time is 1h. After cooling, in an argon environment with a gas pressure of 0.05MPa, the insulation temperature is 500°C, the insulation time is 1h, and the furnace is cooled for more than 4h to prepare the coating.
[0073] Comparative Example 1
[0074] This comparative example is a method for preparing a root canal file without argon high temperature treatment and strengthening treatment, comprising the following steps:
[0075] 1. Preparation of nickel-titanium shape memory alloy
[0076] A CaO crucible with high temperature stability is selected for smelting, and the composition of Ni and Ti is accurate by ensuring that Ti is not oxidized to avoid Ti forming oxides that cause changes in the composition ratio, and a shape memory alloy with a stable NiTi phase transition temperature is obtained. Among them, the molar ratio of titanium metal to nickel metal is 52:48.
[0077] Under inert gas protection and vacuum degree guaranteed to be 10 -2 In a support environment, the initial temperature is first raised to 1200°C, high-temperature refining is performed for 5 minutes, and then the temperature is lowered to 800°C for pouring after standing for 5 minutes. After the nickel-titanium memory alloy is obtained by pouring, it is processed to obtain the required wire material, and the cumulative processing amount is 30%.
[0078] 2. Preparation of surface protective titanium nitride layer
[0079] The nickel-titanium shape memory alloy wire obtained in step 1 is passed through a root canal file processing grinder to grind out a root canal file substrate of the required specifications. The processed root canal file substrate is heat-treated to obtain a root canal file with a surface protective coating. The heat treatment includes: in a nitrogen and argon mixed environment with a gas pressure of 0.05 MPa, a heat preservation temperature of 550°C, and a heat preservation time of 1 hour. After cooling, the coating is obtained.
[0080] Comparative Example 2
[0081] This comparative example is a method for preparing a root canal file without argon high temperature treatment, comprising the following steps:
[0082] 1. Select a CaO crucible with high temperature stability for smelting, ensure that the composition of Ni and Ti is accurate by ensuring that Ti is not oxidized to avoid Ti forming oxides that cause changes in the composition ratio, and obtain a shape memory alloy with a stable NiTi phase transition temperature. Among them, the molar ratio of titanium metal to nickel metal is 52:48.
[0083] Under inert gas protection and vacuum degree guaranteed to be 10 -2 In a support environment, the initial temperature is first raised to 1200°C, high-temperature refining is performed for 5 minutes, and then the temperature is lowered to 800°C for pouring after standing for 5 minutes. After the nickel-titanium memory alloy is obtained by pouring, it is processed to obtain the required wire material, and the cumulative processing amount is 30%.
[0084] 2. Preparation of surface protective titanium nitride layer
[0085] The nickel-titanium shape memory alloy wire obtained in step 1 is passed through a root canal file processing grinder to grind out a root canal file substrate of the required specifications. The processed root canal file substrate is heat-treated to obtain a root canal file with a surface protective coating. The heat treatment includes: in a nitrogen and argon mixed environment with a gas pressure of 0.05 MPa, a heat preservation temperature of 550°C, and a heat preservation time of 1 hour. After cooling, the coating is obtained.
[0086] 3. Strengthening treatment
[0087] The root canal file was subjected to tensile deformation to 5% at room temperature and then unloaded, and this operation was repeated 10 times. Next, the file was subjected to a heat preservation treatment in an inert gas environment at 400° C. for 8 hours.
[0088] Comparative Example 3
[0089] This comparative example is a method for preparing a root canal file without strengthening treatment, comprising the following steps:
[0090] 1. Preparation of nickel-titanium shape memory alloy
[0091] A CaO crucible with high temperature stability is selected for smelting, and the composition of Ni and Ti is accurate by ensuring that Ti is not oxidized to avoid Ti forming oxides that cause the composition ratio to change, and a shape memory alloy with a stable NiTi phase transition temperature is obtained. Among them, the molar ratio of titanium metal to nickel metal is 58:42.
[0092] Under inert gas protection and vacuum degree guaranteed to be 10 -2 In a support environment, the initial temperature is first raised to 1200°C, high-temperature refining is performed for 5 minutes, and then the temperature is lowered to 800°C for pouring after standing for 5 minutes. After the nickel-titanium memory alloy is obtained by pouring, it is processed to obtain the required wire material, and the cumulative processing amount is 30%.
[0093] 2. Preparation of surface protective titanium nitride layer
[0094] The nickel-titanium shape memory alloy wire obtained in step 1 is passed through a root canal file processing grinder to grind out a root canal file substrate of the required specifications. The processed root canal file substrate is heat-treated to obtain a root canal file with a surface protective coating. The heat treatment includes: in a nitrogen and argon mixed environment with a gas pressure of 0.05MPa, the insulation temperature is 550°C, and the insulation time is 1h. After cooling, in an argon environment with a gas pressure of 0.05MPa, the insulation temperature is 500°C, the insulation time is 1h, and the furnace is cooled for more than 4h to prepare the coating.
[0095] 3. Strengthening treatment
[0096] The obtained root canal file was stretched to 5% at room temperature and then unloaded, and this operation was repeated 10 times.
[0097] Test Case
[0098] The amount of Ni ions dissolved in the leaching solution of each group of test pieces after soaking for different times. After soaking for 1 and 10 days, the amount of Ni ions dissolved in each embodiment and comparative example group was significantly reduced compared with the control (nickel-titanium group) without titanium nitride layer. Among them, the amount of Ni ions dissolved in each embodiment was further reduced compared with the comparative example, and there was a statistical difference (all P<0.05).
[0099] Table 1 - Test results of specimens
[0100]
[0101] Note: The fatigue test condition is 90 degrees fatigue 1500 times.
[0102] Although the present invention has been described with reference to exemplary embodiments, it should be understood that the present invention is not limited to the disclosed exemplary embodiments. Various adjustments or changes may be made to the exemplary embodiments of the present specification without departing from the scope or spirit of the present invention. The scope of the claims should be based on the broadest interpretation to cover all modifications and equivalent structures and functions.
Claims
1. A root canal file with better safety, characterized in that: The invention comprises a root canal file base and a titanium nitride layer located on the surface of the root canal file base, wherein the titanium nitride layer is golden yellow on the surface and is evenly and densely coated on the root canal file base. The root canal file with better safety is prepared by the following steps: a. Smelting titanium metal and nickel metal under non-oxidizing conditions, then heating them to 1200-1400°C for refining under inert gas protection or vacuum environment, and then cooling them to 600-1000°C for casting to obtain nickel-titanium memory alloy, and processing them to obtain wire; b. The wire is processed by a root canal file, and the root canal file substrate of the required specifications is ground, and the nitrogen-containing mixed gas environment is maintained for 0.5-5 hours at a gas pressure of 0.005 to 0.1 Mpa and a temperature of 550-600 ℃ to form a titanium nitride layer, and after cooling, the argon environment is maintained at 500-550 ℃ for 0.5-5 hours, and then furnace cooled; Wherein, before or after step b, a strengthening step is further included, wherein the strengthening step includes stretching the wire or root canal file to deform by 1-6%, unloading, repeating the stretching and unloading 5-20 times, and treating in an inert gas environment at 300-550° C. for 1-10 hours.
2. The root canal file with better safety according to claim 1, characterized in that: The titanium nitride layer of the root canal file is good and has no cracks under the fatigue test condition of 90 degrees fatigue 1500 times.
3. The root canal file with better safety according to claim 2, characterized in that: The presence of the titanium nitride layer makes the nickel ion dissolution amount of the root canal file lower than 0.025 μg / L in 10 days.
4. The root canal file with better safety according to claim 3, characterized in that: The molar ratio of titanium metal to nickel metal in the root canal file matrix is 50:50 to 55:
45.
5. The root canal file with better safety according to claim 1, characterized in that: The inert gas used in the strengthening step includes argon and / or helium.
6. The root canal file with better safety according to claim 1, characterized in that: The nitrogen-containing mixed gas includes nitrogen and argon.
7. The root canal file with better safety according to claim 6, characterized in that: The volume ratio of the nitrogen gas to the argon gas is 0.8:1 to 1:0.
8.
8. The root canal file with better safety according to claim 7, characterized in that: The cumulative amount of wire processing is controlled to be 17-60%.