Composite semipermeable membrane

By designing a separation functional layer with a specific structure in the composite semipermeable membrane, and forming a crosslinked polyamide by interfacial polycondensation reaction, the problem of insufficient water permeability under low pressure in the prior art is solved, and efficient freshwatering effect is achieved.

CN117177806BActive Publication Date: 2024-12-03TORAY INDUSTRIES INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202280030036.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-04-22
Filing Date
2022-04-22
Publication Date
2024-12-03
Estimated Expiration
2042-04-22

AI Technical Summary

Technical Problem

The existing composite semipermeable membranes have insufficient water permeability during low pressure operation, making it difficult to meet the demand for efficient fresh waterization.

Method used

A composite semipermeable membrane is designed, which includes a support film and a separation functional layer. The separation functional layer has multiple protrusions, the maximum width of the protrusion to the root width ratio is greater than 1.3, the average density is more than 10 pieces/μm, and the protrusion height ratio is Moderately, a crosslinked polyamide structure is formed through interfacial polycondensation reaction to improve water permeability.

Benefits of technology

It achieves excellent water-making performance under low-pressure operation, improves the water permeability and desalination properties of the membrane, and ensures the stability and durability of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117177806B_ABST
    Figure CN117177806B_ABST
Patent Text Reader

Abstract

The present invention relates to a composite semipermeable membrane, which is a composite semipermeable membrane comprising a supporting membrane and a separation functional layer arranged on the supporting membrane, wherein the separation functional layer has a plurality of protrusions formed by a thin film, and in cross-sections of any 10 locations with a length of 2.0 μm in the membrane surface direction of the supporting membrane, for at least a portion of the plurality of protrusions, the ratio (Wa / Wb) of the maximum width Wa of the protrusions to the root width Wb of the protrusions is greater than 1.3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite semipermeable membrane useful for selective separation of liquid mixtures. The composite semipermeable membrane obtained by the present invention can be used, for example, for desalination of seawater or salt water. Background Art

[0002] Regarding separation of mixtures, there are various technologies for removing substances (such as salts) dissolved in solvents (such as water). In recent years, the use of membrane separation methods has been expanding as a process for energy conservation and resource saving. The membranes used in membrane separation methods include microfiltration membranes, ultrafiltration membranes, nanofiltration membranes, reverse osmosis membranes, etc. These membranes are used, for example, in the case of obtaining drinking water from seawater, salt water, water containing harmful substances, etc., the production of industrial ultrapure water, wastewater treatment, and the recovery of valuable substances.

[0003] In particular, as a reverse osmosis membrane and a nanofiltration membrane, a composite semipermeable membrane having a cross-linked polyamide as a separation active layer has been proposed. As a method for producing a composite semipermeable membrane having a cross-linked polyamide as a separation active layer, there are methods of polymerizing in the presence of an organic additive (Patent Documents 1 and 2), a method of polymerizing in the presence of a monofunctional acyl halide (Patent Document 3), and a method of polymerizing in the presence of a partially hydrolyzed acyl halide (Patent Document 4).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 08-224452

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 6-47260

[0008] Patent Document 3: Japanese Patent Application No. 2014-521499

[0009] Patent Document 4: International Publication No. 2010 / 120326 Summary of the invention

[0010] Problems to be solved by the invention

[0011] Despite the various proposals described above, conventional composite semipermeable membranes still have room for improvement in terms of water permeability during low-pressure operation. An object of the present invention is to provide a composite semipermeable membrane that exhibits excellent water-generating properties even during low-pressure operation.

[0012] Means for solving problems

[0013] In order to achieve the above-mentioned object, the present invention adopts the following configuration.

[0014] [1] A composite semipermeable membrane comprising a supporting membrane and a separation functional layer provided on the supporting membrane, wherein:

[0015] The separation function layer has a plurality of protrusions formed of a thin film,

[0016] In any 10 cross sections of the supporting film having a length of 2.0 μm in the film surface direction, a ratio (Wa / Wb) of a maximum width Wa of the protrusion to a base width Wb of the protrusion of at least a part of the plurality of protrusions is greater than 1.3.

[0017] [2] The composite semipermeable membrane according to [1], wherein the separation functional layer has protrusions having a maximum diameter R of a circle accommodated inside of 30 nm or more.

[0018] [3] The composite semipermeable membrane according to [1] or [2], wherein the average number density of the protrusions in the separation functional layer is 10 or more / μm and 20 or less / μm.

[0019] [4] The composite semipermeable membrane according to [3], wherein an actual length L of the thin film per 1 μm of the supporting membrane in the membrane surface direction of the thin film is 3.0 μm or more,

[0020] The thickness of the thin film is greater than 15 nm.

[0021] [5] The composite semipermeable membrane according to [4], wherein, among the plurality of protrusions, the ratio of the number of protrusions having a height of 200 nm or more to the number of protrusions having a height of 10 nm or more is 1 / 20 or more and 1 / 2 or less.

[0022] [6] The composite semipermeable membrane as described in [4] or [5], wherein, among the plurality of protrusions, the ratio of the number of protrusions having a height of 400 nm or more to the number of protrusions having a height of 10 nm or more is 1 / 20 or more and 1 / 5 or less.

[0023] Effects of the Invention

[0024] According to the present invention, it is possible to obtain a composite semipermeable membrane having excellent water generating performance even in low-pressure operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] [ Figure 1 ] Figure 1 This is a cross-sectional view of a composite semipermeable membrane according to one embodiment of the present invention.

[0026] [ Figure 2 ] Figure 2 This is a cross-sectional view showing the corrugated structure of the thin film in the separation functional layer.

[0027] [ Figure 3] Figure 3 is a cross-sectional view of the corrugated structure and is a schematic diagram showing the height of the protrusions.

[0028] [ Figure 4 ] Figure 4 This is an enlarged cross-sectional view of a protrusion in the wrinkle structure. DETAILED DESCRIPTION

[0029] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these embodiments.

[0030] It should be noted that, in the present specification, "weight" and "mass", and "weight %" and "mass %" are treated as synonyms, respectively.

[0031] The numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0032] 1. Composite semipermeable membrane

[0033] The composite semipermeable membrane of the present embodiment includes a supporting membrane and a separation functional layer provided on the supporting membrane.

[0034] (1-1) Supporting film

[0035] In this embodiment, the supporting membrane does not substantially have separation performance such as ions, and strength is imparted to the separation functional layer that substantially has separation performance. The size and distribution of the pores of the supporting membrane are not particularly limited, but it is preferred that the supporting membrane has uniform and fine pores, or fine pores that gradually increase in size from the surface on one side where the separation functional layer is formed to the other side, and the size of the fine pores on the surface on the side where the separation functional layer is formed is 0.1 nm or more and 100 nm or less.

[0036] The material and shape of the supporting film are not particularly limited. Figure 1 As shown, the supporting membrane may be a composite membrane including a substrate 2 and a porous supporting layer 3 provided on the substrate 2, or may be a membrane consisting of only one layer.

[0037] As the substrate, for example, a cloth having at least one selected from polyester or aromatic polyamide as a main component can be exemplified. As the cloth, a long-fiber nonwoven fabric or a short-fiber nonwoven fabric can be preferably used.

[0038] The thickness of the substrate is preferably in the range of 10 μm to 200 μm, and more preferably in the range of 30 μm to 120 μm.

[0039] The porous supporting layer may, for example, contain at least one polymer selected from the group consisting of polysulfone; polyethersulfone; polyamide; polyester; cellulose polymers such as cellulose acetate and cellulose nitrate; vinyl polymers such as polyethylene, polypropylene, polyvinyl chloride, and polyacrylonitrile, homopolymers such as polyphenylene sulfide, polyphenylene sulfide sulfone, polyphenylene sulfone and polyphenylene ether, and their copolymers.

[0040] Among them, polysulfone, cellulose acetate, polyvinyl chloride, or a mixture thereof is preferably used for the porous supporting layer, and polysulfone having high chemical stability, mechanical stability, and thermal stability is particularly preferably used.

[0041] In addition, the thickness of the porous supporting layer is preferably in the range of 10 to 200 μm, more preferably in the range of 20 to 100 μm. By making the thickness of the porous supporting layer 10 μm or more, good pressure resistance can be obtained, and a uniform supporting membrane without defects can be obtained, and a composite semipermeable membrane having such a porous supporting layer can show good desalination performance. By making the thickness of the porous supporting layer 200 μm or less, the residual amount of unreacted substances during manufacturing will not increase, and the reduction of chemical resistance caused by the reduction of permeate water can be prevented.

[0042] In order to obtain sufficient mechanical strength and packing density of the composite semipermeable membrane, the thickness of the supporting membrane is preferably in the range of 30 to 300 μm, more preferably in the range of 50 to 250 μm.

[0043] The morphology of the support film can be observed by a scanning electron microscope, a transmission electron microscope, an interatomic microscope, etc. For example, if the morphology of the support film is observed by a scanning electron microscope, after the porous support layer is peeled off from the substrate, it is cut by a freeze fracture method to prepare a sample for cross-sectional observation. The sample is preferably thinly coated with platinum or platinum-palladium or ruthenium tetrachloride, more preferably ruthenium tetrachloride, and observed with a high-resolution field emission scanning electron microscope (UHR-FE-SEM) at an accelerating voltage of 3 to 6 kV.

[0044] The thickness of the above-mentioned substrate, porous supporting layer and composite semipermeable membrane can be measured using a digital thickness gauge. In addition, since the thickness of the separation functional layer described later is very thin compared to the supporting membrane, the thickness of the composite semipermeable membrane can also be regarded as the thickness of the supporting membrane. Therefore, by measuring the thickness of the composite semipermeable membrane with a digital thickness gauge, and deducting the thickness of the substrate from the thickness of the composite semipermeable membrane, the thickness of the porous supporting layer can be easily calculated. When using a digital thickness gauge, preferably 20 places are measured for thickness and average value is calculated.

[0045] It should be noted that the thickness of the substrate, porous supporting layer, and composite semipermeable membrane can be measured by the above-mentioned microscope. For one sample, the thickness is measured by electron micrographs of cross-section observations of any five positions, and the average value is calculated to obtain the thickness. It should be noted that the thickness and pore size in the present embodiment refer to the average value.

[0046] (1-2) Separation functional layer

[0047] In a composite semipermeable membrane, the separation functional layer is the one that actually has the ability to separate ions, etc. Figure 1 In the cross-sectional view of the composite semipermeable membrane 1, the separation functional layer is marked with a mark "4" to indicate that the separation functional layer is Figure 2 As shown, there are a plurality of protrusions formed by the film 11 .

[0048] The separation functional layer preferably contains polyamide as a main component. In the case of a separation functional layer with polyamide as a main component, the polyamide can be formed, for example, by interfacial polycondensation of a polyfunctional amine and a polyfunctional acyl halide. Here, it is preferred that at least one of the polyfunctional amine or the polyfunctional acyl halide contains a compound having three or more functions.

[0049] In order to obtain sufficient separation performance and permeate amount, the thickness of the separation functional layer is usually in the range of 0.01 to 1 μm, preferably in the range of 0.1 to 0.5 μm.

[0050] Here, the polyfunctional amine refers to an amine having at least two primary and / or secondary amino groups in one molecule, at least one of which is a primary amino group. Examples of the polyfunctional amine include aromatic polyfunctional amines such as phenylenediamine, phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 3-aminobenzylamine, and 4-aminobenzylamine, in which two amino groups are bonded to a benzene ring in any positional relationship of ortho, meta, or para positions, aliphatic amines such as ethylenediamine and propylenediamine, and alicyclic polyfunctional amines such as 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, 4-aminopiperidine, and 4-aminoethylpiperazine.

[0051] Among them, if the selective separation, permeability and heat resistance of the membrane are taken into consideration, aromatic polyfunctional amines having 2 to 4 primary and / or secondary amino groups in one molecule are preferred. As such polyfunctional aromatic amines, for example, m-phenylenediamine, p-phenylenediamine, 1,3,5-triaminobenzene, etc. are preferably used. Among them, m-phenylenediamine (hereinafter referred to as m-PDA) is more preferably used from the perspective of ease of acquisition and ease of operation.

[0052] These multifunctional amines can be used alone or in combination of two or more. When two or more are used in combination, the above amines can be combined with each other or with an amine having at least two secondary amino groups in one molecule. Examples of amines having at least two secondary amino groups in one molecule include piperazine and 1,3-bispiperidinylpropane.

[0053] The polyfunctional acid halide refers to an acid halide having at least two halogenated carbonyl groups in one molecule. Examples of the trifunctional acid halide include trimesoyl chloride, 1,3,5-cyclohexanetricarboxyl chloride, and 1,2,4-cyclobutanetricarboxyl chloride. Examples of the bifunctional acid halide include aromatic bifunctional acid halides such as biphenyl dicarboxyl chloride, azophthaloyl chloride, terephthaloyl chloride, isophthaloyl chloride, and naphthalene dicarboxyl chloride, aliphatic bifunctional acid halides such as adipoyl chloride and sebacoyl chloride, and alicyclic bifunctional acid halides such as cyclopentane dicarboxyl chloride, cyclohexane dicarboxyl chloride, and tetrahydrofuran dicarboxyl chloride.

[0054] If the reactivity with polyfunctional amines is considered, the polyfunctional acyl halide is preferably a polyfunctional acyl chloride. In addition, if the selective separation and heat resistance of the membrane are considered, a polyfunctional aromatic acyl chloride having 2 to 4 phosgene groups in one molecule is more preferably used. Among them, from the viewpoint of ease of acquisition and ease of operation, trimesoyl chloride is more preferably used as the polyfunctional acyl halide. These polyfunctional acyl halides can be used alone or in combination of two or more.

[0055] In addition, in the separation functional layer, such as Figure 2 As shown, the film forms a wrinkled structure with multiple concave and convex parts. Hereinafter, "convex part" and "concave part" refer to relatively protruding parts and concave parts in the film, and in particular, the part above (in the direction away from the supporting film) relative to the reference line A described later is called a convex part, and the part below (on the supporting film side) is called a concave part. "Protrusion" refers to the bottom of the concave part to the bottom of the adjacent concave part, that is, to the bottom of the two adjacent concave parts of one convex part. In addition, in this specification, a protrusion refers to a protrusion having a height of more than 1 / 5 of the 10-point average surface roughness of the film.

[0056] The separation functional layer in this embodiment preferably has an actual length L of the thin film of the supporting membrane per 1 μm length in the membrane surface direction of the supporting membrane of 3.0 μm or more. By making the actual length L of the thin film 3.0 μm or more, the composite semipermeable membrane can obtain high water permeability. The actual length L of the thin film is more preferably 3.0 to 100 μm, and further preferably 3.0 to 10 μm.

[0057] It should be noted that, in the present specification, the “film surface direction” refers to a direction orthogonal to a direction perpendicular to the film surface.

[0058] The actual length L of the film can be calculated by a general method for calculating the surface area or specific surface area. The method is not particularly limited, and examples thereof include methods using electron microscopes such as a scanning electron microscope (SEM, FE-SEM) and a transmission electron microscope (TEM).

[0059] The following is a method for measuring the actual length L of a thin film obtained using a transmission electron microscope (TEM). First, in order to prepare ultrathin sections for TEM, a sample is embedded in a water-soluble polymer. As a water-soluble polymer, any polymer can be used as long as it can maintain the shape of the sample, and an example of such polymer is PVA.

[0060] Next, in order to easily observe the cross section, it was stained with OsO4 and cut with an ultrathin slicer to make ultrathin sections. The cross-sectional photographs of the obtained ultrathin sections were taken using an electron microscope. The observation magnification can be appropriately determined according to the film thickness of the separation functional layer, but in order to be able to observe the cross-sectional shape of the separation functional layer and not make the measurement local, if the thickness of the separation functional layer is about 10 to 100 nm, the observation magnification can be set to 50,000 to 100,000 times.

[0061] In the cross-sectional photograph obtained above, the actual length of the thin film of the supporting membrane in the membrane surface direction was measured for each 1 μm length in any 10 cross-sectional locations with a length of 2.0 μm, and the arithmetic mean was calculated as the actual length L of the thin film in the composite semipermeable membrane.

[0062] The 10-point average surface roughness of the film was obtained by the following method.

[0063] The cross section perpendicular to the film surface is observed by electron microscopy. The observation magnification is preferably 10,000 to 100,000 times. In the obtained cross-sectional image, Figure 2 As shown, a thin film (on Figure 2 The surface of the surface of the roughness curve is represented as a curve. For the curve, the roughness curve defined according to ISO4287:1997 is determined. Also based on ISO4287:1997, the average line of the roughness curve is obtained. The average line is a straight line drawn in a manner that the total area of ​​the area surrounded by the average line and the roughness curve is equal above and below the average line.

[0064] In the cross-sectional image with a length of 2.0 μm in the direction of the average line obtained above, the average line is used as the reference line A. For the 5 convex parts from the highest convex part to the 5th height, the height from the reference line (the distance from the reference line to the apex of the convex part) H1 to H5 is measured, and the average value is calculated. In addition, for the 5 concave parts from the deepest concave part to the 5th depth, the depth (the distance from the reference line to the apex of the concave part) D1 to D5 is measured, and the average value is calculated. The sum of the two average values ​​obtained is the 10-point average surface roughness. It should be noted that the vertex refers to the point where the distance from the reference line is the largest in the convex part or concave part.

[0065] The height of the protrusion is calculated as follows: In the cross section with a length of 2.0 μm in the direction of the above average line, for protrusions with a surface roughness of 1 / 5 or more of the above 10-point average, the sum of the average d of the depths of the concave portions (the distance from the reference line to the vertex of the concave portion) d1 and d2 at both ends of the protrusion and the height h of the convex portion (the distance from the reference line to the vertex of the convex portion) is calculated as the protrusion height Ph.

[0066] In the present embodiment, in the cross section of any 10 parts with a length of 2.0 μm in the direction of the average line, the ratio (N / M) of the number of protrusions N with a height of 200 nm or more present in the cross section of the 10 parts relative to the number of protrusions M with a height of 10 nm or more present in the cross section of the 10 parts is preferably 1 / 20 or more and 1 / 2 or less. By making N / M more than 1 / 20, a composite semipermeable membrane with high water permeability can be obtained. N / M is more preferably more than 1 / 10. In addition, by making N / M less than 1 / 2, high water permeability can be obtained. N / M is more preferably less than 1 / 3.

[0067] It should be noted that the number of protrusions existing in the cross sections at 10 locations refers to the number of protrusions included in each cross section calculated in all the cross sections at 10 locations, and the total number of protrusions calculated in each cross section is added up in all the cross sections at 10 locations.

[0068] In addition, in the present embodiment, in the cross-section of 10 parts with a length of 2.0 μm in the direction of the average line, among all the protrusions in the cross-section of any 10 parts, it is preferred to have at least one protrusion with a height of 400 nm or more. In addition, the ratio (N1 / M) of the number of protrusions N1 with a height of 400 nm or more present in the cross-section of 10 parts relative to the number of protrusions M with a height of 10 nm or more present in the cross-section of 10 parts is more preferably 1 / 20 or more and 1 / 5 or less. By having protrusions with a height of 400 nm or more in the above range, a composite semipermeable membrane with high water permeability can be obtained.

[0069] The inventors of the present application have conducted intensive research and found that, by making at least a portion of the plurality of protrusions of the separation functional layer have a length of 2.0 μm in the membrane surface direction of the support membrane, in the cross section of any 10 locations, Figure 4 As shown in FIG. 1 , the ratio (Wa / Wb) obtained by the maximum width Wa of the protrusion and the root width Wb of the protrusion is greater than 1.3, thereby obtaining a composite semipermeable membrane that shows high water permeability even when operating at low pressure. Wa / Wb is preferably greater than 1.4, more preferably greater than 1.6. In addition, in order to achieve the same as the average number density of the protrusions, Wa / Wb is preferably less than 2.0, more preferably less than 1.8, and further preferably less than 1.7.

[0070] The maximum width Wa of the protrusion and the width Wb of the root of the protrusion can be observed by a scanning electron microscope or a transmission electron microscope. For example, if the maximum width Wa of the protrusion and the width Wb of the root of the protrusion are observed by a scanning electron microscope, platinum or platinum-palladium or ruthenium tetroxide is preferably thinly coated on the composite semipermeable membrane sample, and ruthenium tetroxide is more preferably thinly coated, and observation is performed using a high-resolution field emission scanning electron microscope (UHR-FE-SEM) at an acceleration voltage of 3 to 6 kV.

[0071] A high-resolution field emission scanning electron microscope can use a Hitachi S-900 electron microscope or the like. The observation magnification is preferably 5,000 to 100,000 times. Based on the obtained electron microscope photograph and taking into account the observation magnification, the maximum width Wa of the protrusion and the root width Wb of the protrusion can be directly measured using a ruler or the like. In addition, the maximum width Wa of the protrusion and the root width Wb of the protrusion are both measured as the interval between the inner surfaces of the protrusion. In addition, the root width Wb of the protrusion refers to the interval between the straight lines drawn from the vertices of the concave portions adjacent to the protrusion in a manner orthogonal to the reference line.

[0072] In the cross-sections of any 10 locations with a length of 2.0 μm in the membrane surface direction of the supporting membrane, the ratio of the number of protrusions with Wa / Wb greater than 1.3 in the cross-sections of the 10 locations to the number of all protrusions in the cross-sections of the 10 locations is preferably 20% or more. By making this ratio 20% or more, the water permeability of the composite semipermeable membrane can be improved. This ratio is more preferably 40% or more, and further preferably 50% or more.

[0073] In addition, the separation functional layer in the present embodiment preferably has a maximum diameter of a circle contained in the protrusion, i.e., a protrusion with a filling circle diameter R of 30 nm or more. By having a protrusion with a filling circle diameter R of 25 nm or more, the water permeability of the composite semipermeable membrane is improved. More preferably, it includes a protrusion with a filling circle diameter R of 32 nm or more, and more preferably 35 nm or more. In order to suppress the reduction of the average number density of the protrusion, it is preferred that the filling circle diameter R is 80 nm or less. The filling circle diameter R can be measured by a cross-sectional photograph of the above-mentioned separation functional layer.

[0074] In the cross-sections of any 10 locations with a length of 2.0 μm in the membrane surface direction, the ratio of the number of protrusions having a filling circle diameter R of 25 nm or more present in the cross-sections of the 10 locations to the total number of protrusions present in the cross-sections of the 10 locations is preferably 20% or more, more preferably 40% or more, and even more preferably 50% or more.

[0075] In the separation functional layer of the present embodiment, the average number density of the protrusions is preferably 10 / μm or more, more preferably 12 / μm or more. In addition, the average number density of the protrusions in the separation functional layer is preferably 20 / μm or less.

[0076] By making the average number density of protrusions 10 pieces / μm or more, the composite semipermeable membrane can obtain sufficient water permeability, and further can suppress the deformation of the protrusions during pressure application, and can obtain stable membrane performance. In addition, by making the average number density of protrusions 20 pieces / μm or less, the pleated structure grows sufficiently, and a composite semipermeable membrane with desired water permeability can be easily obtained.

[0077] The average number density of protrusions can be measured by observing cross sections of any 10 locations with a length of 2.0 μm in the film surface direction and by the number of protrusions having one fifth or more of the 10-point average surface roughness in each cross section.

[0078] 2. Manufacturing method

[0079] An example of a method for producing the composite semipermeable membrane according to the present embodiment described above is shown below.

[0080] (2-1) Formation of separation functional layer

[0081] The process of forming a separation functional layer on a supporting membrane is described. Hereinafter, the case where the supporting membrane has a substrate and a porous supporting layer is taken as an example. When the supporting membrane does not include a substrate, "the surface of the porous supporting layer" and "on the porous supporting layer" can be replaced with "the surface of the supporting membrane" and "on the supporting membrane", respectively.

[0082] The process of forming the separation function layer includes the step of contacting a polyfunctional amine solution with a polyfunctional acyl halide solution on the porous support layer to form polyamide through an interfacial polycondensation reaction. More specifically, the process of forming the separation function layer includes:

[0083] (i) a step of contacting the porous supporting layer with a polyfunctional amine solution;

[0084] (ii) After the above step (i), the porous supporting layer is brought into contact with a polyfunctional acid halide solution to thereby form polyamide on the porous supporting layer by interfacial polycondensation.

[0085] Hereinafter, each manufacturing process will be described in detail.

[0086] The polyfunctional amine solution is an aqueous solution, wherein the concentration of the polyfunctional amine in the solution is preferably in the range of 0.1 to 20 wt %, more preferably in the range of 0.5 to 15 wt %. If the concentration of the polyfunctional amine is within the above range, a composite semipermeable membrane having sufficient desalination performance and water permeability can be obtained.

[0087] The polyfunctional amine aqueous solution may contain a surfactant, an organic solvent, a basic compound, an antioxidant, and the like, as long as the reaction between the polyfunctional amine and the polyfunctional acid halide is not inhibited.

[0088] Examples of the surfactant include compounds having a polyoxyalkylene structure, a fatty acid ester structure, or a hydroxyl group. Examples of the polyoxyalkylene structure include -(CH2CH2O) n -、-(CH2CH2(CH3)O) n -、-(CH2CH2CH2O) n -、-(CH2CH2CH2CH2O) n - etc. As the fatty acid ester structure, fatty acids with long-chain aliphatic groups can be cited. As the long-chain aliphatic group, any of straight chain and branched chain can be cited, and as fatty acids, stearic acid, oleic acid, lauric acid, palmitic acid and its salts can be cited. In addition, as fatty acid esters derived from oils and fats, for example, beef tallow, palm oil, coconut oil, etc. can also be cited. As surfactants with sulfonic groups, 1-hexanesulfonic acid, 1-octanesulfonic acid, 1-decanesulfonic acid, 1-dodecanesulfonic acid, perfluorobutanesulfonic acid, toluenesulfonic acid, cumenesulfonic acid, octylbenzenesulfonic acid, etc. can be cited. As surfactants with hydroxyl groups, ethylene glycol, propylene glycol, 2-propylene glycol, 1,4-butanediol, glycerol, sorbitol, glucose, sucrose, etc. can be cited. The surfactant has the effect of improving the wettability of the surface of the porous supporting layer and reducing the interfacial tension between the amine aqueous solution and the non-polar solvent.

[0089] Examples of organic solvents include chain amide compounds and cyclic amide compounds. Examples of chain amide compounds include N-methylformamide, N,N-dimethylformamide, N,N,-dimethylacetamide, N,N-diethylformamide, and N,N-diethylacetamide. Examples of cyclic amide compounds include N-methylpyrrolidone, γ-butyrolactam, and ε-caprolactam. Organic solvents sometimes act as catalysts for interfacial polycondensation reactions, and sometimes efficiently perform interfacial polycondensation reactions by addition.

[0090] Examples of the basic compound include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, inorganic carbonate and hydrogen carbonate compounds such as sodium carbonate, sodium hydrogen carbonate, potassium carbonate and potassium hydrogen carbonate, and organic compounds such as tetramethylammonium hydroxide and tetraethylammonium hydroxide.

[0091] Examples of antioxidants include phenolic antioxidants, amine antioxidants, sulfur antioxidants, and phosphorus antioxidants. Examples of phenolic antioxidants (including hindered phenolic antioxidants) include 2,6-di-tert-butyl-4-methylphenol, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), and tetrakis-[methylene-3-(3', 5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane. Examples of amine antioxidants include phenyl-β-naphthylamine, α-naphthylamine, N,N'-di-sec-butyl-p-phenylenediamine, phenothiazine, and N,N'-diphenyl-p-phenylenediamine.

[0092] As sulfur-based antioxidants, there are dilauryl 3,3'-thiodipropionate, distearyl thiodipropionate, lauryl stearyl thiodipropionate, dimyristyl 3,3'-thiodipropionate, etc. As phosphorus-based antioxidants, there are triphenyl phosphite, octadecyl phosphite, and trinonylphenyl phosphite, etc. As other antioxidants, there are ascorbic acid or its alkali metal salts, sterically hindered phenol compounds such as butylated hydroxytoluene and butylated hydroxyanisole, isopropyl citrate, dl-α-tocopherol, nordihydroguaiaretic acid, propyl gallate, etc.

[0093] The contact between the polyfunctional amine aqueous solution and the porous supporting layer is preferably carried out uniformly and continuously on the surface of the porous supporting layer. Specifically, for example, a method of coating the polyfunctional amine aqueous solution on the porous supporting layer or a method of immersing the porous supporting layer in the polyfunctional amine aqueous solution can be mentioned. The contact time between the porous supporting layer and the polyfunctional amine aqueous solution is preferably in the range of 1 to 10 minutes, and more preferably in the range of 1 to 3 minutes.

[0094] After the polyfunctional amine aqueous solution is contacted with the porous supporting layer, it is preferred to fully discharge the liquid in a manner that no droplets remain on the film. By fully discharging the liquid, it is possible to prevent the residual droplets from becoming film defects after the film is formed and reducing the film performance. As a method for discharging the liquid, for example, as described in Japanese Patent Laid-Open No. 2-78428, a method for holding the supporting film after contacting the polyfunctional amine aqueous solution in a vertical direction and allowing the excessive aqueous solution to flow down naturally, a method for forcibly discharging the liquid by blowing air currents such as nitrogen from an air nozzle, etc., can be used. In addition, after the discharge, the film surface can also be dried to remove a portion of the moisture in the aqueous solution.

[0095] Step (ii) is described below. Step (ii) is a step of bringing the porous supporting layer into contact with a polyfunctional acid halide or an organic solvent solution containing a polyfunctional acid halide, thereby generating polyamide on the porous supporting layer by interfacial polycondensation.

[0096] The concentration of the polyfunctional acid halide in the organic solvent solution is preferably in the range of 0.01 to 10% by weight, and more preferably in the range of 0.02 to 2.0% by weight. By setting it to 0.01% by weight or more, a sufficient reaction rate can be obtained, and by making it 10% by weight or less, the occurrence of side reactions can be suppressed.

[0097] The organic solvent is preferably an organic solvent that is immiscible with water, dissolves the polyfunctional acyl halide, and does not damage the supporting membrane, as long as it is inactive to the polyfunctional amine compound and the polyfunctional acyl halide. Preferred examples of the organic solvent include hydrocarbon compounds such as n-hexane, n-octane, n-nonane, n-decane, n-undecane, n-dodecane, isodecane, and isododecane.

[0098] The polyfunctional acid halide solution preferably contains water. When the polyfunctional acid halide solution contains water, the above-mentioned shape of the protrusion can be realized. The amount of water contained in the polyfunctional acid halide solution is preferably in the range of 1 to 500 ppm, more preferably in the range of 1 to 200 ppm.

[0099] The polyfunctional acid halide solution may contain a compound represented by the chemical formula (I) (hereinafter referred to as compound (I)).

[0100] [Chemical formula 1]

[0101]

[0102] In the above formula, R1 and R2 are each independently an alkyl group having 1 or more carbon atoms.

[0103] As compound (I), aromatic esters are preferred, and phthalates are particularly preferred. As compound (I), specifically, dibutyl phthalate, dibutyl benzyl phthalate, diethylhexyl phthalate, diisodecyl phthalate, diisooctyl phthalate, dioctyl phthalate, diisobutyl phthalate, diethyl phthalate, dimethyl phthalate, diisooctyl phthalate, dipropyl phthalate, dicyclohexyl phthalate, dinonyl phthalate, diphenyl phthalate, dihexyl phthalate, dibenzyl phthalate, diphenyl phthalate, and bis(2-ethylhexyl)phthalate can be cited.

[0104] The concentration of the compound (I) in the polyfunctional acid halide solution may vary depending on the type of compound (I) added, but is preferably within a range of 5 ppm to 500 ppm.

[0105] Examples of a method for bringing the organic solvent solution containing the polyfunctional acid halide into contact with the polyfunctional amine compound aqueous solution include coating and dropping.

[0106] In step (ii), a layer of a polyfunctional acid halide solution is formed above the layer of the polyfunctional amine aqueous solution on the porous supporting layer. Here, in the layer of the polyfunctional acid halide solution, a gradient is preferably formed in which the water content increases as the layer approaches the porous supporting layer.

[0107] By forming the above-mentioned gradient immediately after the layer of the polyfunctional amine aqueous solution and the layer of the polyfunctional acyl halide solution are brought into contact (approximately within 5 seconds), a surface tension difference is generated inside the layer of the polyfunctional acyl halide solution, and a flow is generated in the layer of the polyfunctional acyl halide solution. By this flow, protrusions with a shape in which the base of the protrusions is thin and the main body is swollen are formed in the pleated structure of the separation functional layer, which can improve the water permeability of the composite semipermeable membrane.

[0108] The above-mentioned gradient can be formed, for example, by applying a polyfunctional acid halide solution having different water contents on the porous support layer multiple times. The number of applications is preferably 2 times. The water content contained in the polyfunctional acid halide solution applied first (the first polyfunctional acid halide solution) is preferably 10 to 500 ppm, more preferably 10 to 200 ppm. The water content contained in the polyfunctional acid halide solution applied for the second time (the second polyfunctional acid halide solution) is preferably 1 to 300 ppm, more preferably 1 to 150 ppm.

[0109] When forming a separation functional layer comprising a cross-linked polyamide by interfacial polycondensation, by carrying out the process in the presence of compound (I), the actual length of the film of the separation functional layer can be increased, and a separation functional layer having a large film thickness can be formed, thereby obtaining a composite semipermeable membrane showing high water permeability.

[0110] The mechanism of action of compound (I) is not clear, and it is believed that the interaction between the aromatic rings present in compound (I) and the aromatic rings present in the polyamide during the formation process has an effect. In detail, it is believed that in the interfacial polycondensation of polyfunctional amines and polyfunctional acyl halides, when the amine diffuses from the polyfunctional amine aqueous solution side to the organic solvent side containing the polyfunctional acyl halide, due to the presence of compound (I), the concentration gradient of the amine slows down, and as a result, the formation time of the protrusions in the separation functional layer becomes sufficiently long, the structural formation of the protrusions is easy to proceed, and the surface area of ​​the protrusions and the thickness of the film are increased.

[0111] At this time, by forming a liquid flow in the layer of the polyfunctional acid halide solution, that is, the layer of the organic solvent, the formation of the protrusions can be further promoted, a shape with a thin base and a swollen body can be obtained, and the height of the protrusions can be increased.

[0112] By making the protrusions of the separation functional layer have a thin base, a bulging body, and a large height, it is possible to reduce the contact area with adjacent protrusions while ensuring the specific surface area, thereby ensuring the effective membrane area and achieving higher water permeability.

[0113] The temperature of the membrane surface immediately after the polyfunctional amine aqueous solution and the polyfunctional acyl halide solution are brought into contact is preferably in the range of 25 to 60° C., and more preferably in the range of 30 to 50° C. By making the temperature of the membrane surface above 25° C., the pleated structure grows significantly, and the permeation flux is improved. In addition, by making the temperature of the membrane surface below 60° C., a composite semipermeable membrane showing a good salt removal rate can be obtained.

[0114] The method of applying temperature to the membrane surface may be to heat the support membrane or to contact the support membrane with a heated organic solvent solution of the polyfunctional acyl halide. The temperature of the membrane surface immediately after the polyfunctional amine aqueous solution and the polyfunctional acyl halide solution are contacted can be measured by a non-contact thermometer such as a radiation thermometer.

[0115] As described above, an organic solvent solution of a polyfunctional acyl halide is brought into contact with an aqueous solution of a polyfunctional amine to perform interfacial polycondensation, and after a separation functional layer comprising a cross-linked polyamide is formed on a porous support layer, the remaining solvent can be removed. The method of draining the liquid can be, for example, a method in which the membrane is held in a vertical direction and the excess organic solvent is removed by naturally flowing down. In this case, the time for holding in the vertical direction is preferably 1 to 5 minutes, and more preferably 1 to 3 minutes. By making the time more than 1 minute, a sufficient amount of polyamide can be formed as a separation functional layer, and by making the time less than 5 minutes, the organic solvent will not evaporate excessively, and the generation of membrane defects can be suppressed.

[0116] (2-2) Formation of Support Film

[0117] As the supporting membrane, a commercially available filter can be used. Alternatively, a supporting membrane having a substrate and a porous supporting layer can be formed by coating a polymer solution on a substrate and then solidifying the polymer, or by coating a polymer solution on a substrate such as glass, then solidifying the polymer, and then peeling the polymer from the substrate.

[0118] For example, when polysulfone is used to form a supporting membrane, a polymer solution is obtained by dissolving polysulfone in N,N-dimethylformamide (hereinafter referred to as DMF), applying the solution to a certain thickness on a substrate, and wet coagulating it in water. According to this method, a porous supporting layer having fine pores with a diameter of several tens of nanometers or less on most of the surface can be obtained.

[0119] (2-3) Other treatments

[0120] By subjecting the composite semipermeable membrane after forming the separation functional layer to a hot water treatment step preferably at 50 to 150° C., more preferably at 70 to 130° C., for preferably 1 second to 10 minutes, more preferably 1 minute to 8 minutes, the desalination performance and water permeability can be improved.

[0121] In addition, the salt removal rate of the composite semipermeable membrane can be further improved by a process including contacting the composite semipermeable membrane with a compound (A) which reacts with the primary amino group on the separation functional layer to form a diazonium salt or its derivative after hot water treatment, and then contacting the composite semipermeable membrane with a water-soluble compound (B) which is reactive with the above-mentioned compound (A).

[0122] As a compound (A) that reacts with a primary amino group to generate a diazonium salt or a derivative thereof, aqueous solutions of nitrous acid and its salts, nitrosyl compounds, etc. can be cited. Since aqueous solutions of nitrous acid and nitrosyl compounds are prone to produce gas and decompose, it is preferred that nitrous acid is generated successively, for example, by the reaction of nitrite with an acidic solution. Generally speaking, nitrite reacts with hydrogen ions to generate nitrous acid (HNO2), but it can be efficiently generated under the conditions of preferably less than 7 pH of the aqueous solution, more preferably less than 5, and further preferably less than 4. Among them, from the perspective of simplicity of operation, an aqueous solution of sodium nitrite reacting with hydrochloric acid or sulfuric acid in an aqueous solution is particularly preferred.

[0123] As the compound (A) that reacts with the primary amino group to form a diazonium salt or a derivative thereof, for example, when sodium nitrite is used, the concentration of sodium nitrite is preferably in the range of 0.01 to 1% by weight. If the sodium nitrite is within the above range, the effect of generating sufficient diazonium salt or a derivative thereof can be obtained, and the solution is also easy to handle.

[0124] The temperature of the compound is preferably 15° C. to 45° C. Within this range, the reaction does not take too much time, the decomposition of nitrous acid does not occur too quickly, and the operation is easy.

[0125] The contact time between the primary amino group and the compound is sufficient as long as the diazonium salt and / or its derivative is generated. If the concentration is high, the treatment can be carried out in a short time, but if the concentration is low, a long time is required. Therefore, the solution of the above concentration is preferably within 10 minutes, more preferably within 3 minutes.

[0126] In addition, the method for contacting the primary amino group with the compound is not particularly limited, and the solution of the compound may be applied (coating), or the composite semipermeable membrane may be immersed in the solution of the compound. Any solvent may be used as long as the compound is dissolved and the composite semipermeable membrane is not corroded. In addition, the solution of the compound may contain a surfactant, an acidic compound, a basic compound, etc. as long as it does not hinder the reaction between the primary amino group and the reagent.

[0127] Next, the composite semipermeable membrane having the diazonium salt or its derivative is contacted with a water-soluble compound (B) that reacts with the diazonium salt or its derivative. Examples of the water-soluble compound (B) that reacts with the diazonium salt or its derivative include chloride ions, bromide ions, cyanide ions, iodide ions, fluoroboric acid, hypophosphorous acid, sodium bisulfite, sulfite ions, aromatic amines, phenols, hydrogen sulfide, thiocyanic acid, and the like.

[0128] When reacting with sodium bisulfite and sulfite ions, a substitution reaction occurs instantly, and the amino group is replaced by a sulfonic group. In addition, by contacting with aromatic amines and phenols, a diazo coupling reaction occurs, and aromatic groups can be introduced into the membrane surface.

[0129] These compounds may be used alone or in combination, or may be contacted with different compounds multiple times. As the compound to be contacted with the composite semipermeable membrane having the diazonium salt or its derivative formed, sodium bisulfite and sulfite ion are preferred.

[0130] In order to obtain the desired effect, the concentration and time of contact between the composite semipermeable membrane having the diazonium salt or its derivative formed therein and the water-soluble compound (B) reactive with the diazonium salt or its derivative can be appropriately adjusted.

[0131] The temperature at which the composite semipermeable membrane having the diazonium salt or its derivative is contacted with the water-soluble compound (B) that reacts with the diazonium salt or its derivative is preferably 10 to 90° C. When the contact temperature is within the above range, the reaction proceeds easily, and on the other hand, a decrease in the amount of permeated water due to shrinkage of the polymer is not caused.

[0132] It should be noted that the membrane before and after the treatment in this column (2-3) is referred to as a "composite semipermeable membrane", and the layer on the supporting membrane in the membrane before and after the treatment in this column (2-3) is referred to as a "separation functional layer".

[0133] (3) Utilization of composite separation membranes

[0134] The composite semipermeable membrane of the present embodiment manufactured in this way is wound around a cylindrical water collecting pipe having a plurality of holes together with raw water flow path materials such as plastic nets, permeated water flow path materials such as tricot fabrics, and a membrane for improving pressure resistance as needed, and is suitable for use as a spiral composite semipermeable membrane element. Furthermore, a composite semipermeable membrane module in which the element is connected in series or in parallel and housed in a pressure vessel can also be made.

[0135] In addition, the above-mentioned composite semipermeable membrane, its elements, and modules can be combined with a pump for supplying raw water thereto, a device for pre-treating the raw water, etc. to form a fluid separation device. By using this separation device, raw water can be separated into permeated water such as drinking water and concentrated water that has not passed through the composite semipermeable membrane, thereby obtaining water that meets the purpose.

[0136] When the operating pressure of the fluid separation device is high, the salt removal rate increases, but the energy required for operation also increases. In addition, considering the durability of the composite semipermeable membrane, it is preferred that the operating pressure when the treated water passes through the composite semipermeable membrane is above 0.5 MPa and below 10 MPa.

[0137] When the temperature of the supply water increases, the salt removal rate of the composite semipermeable membrane decreases, but as the temperature decreases, the membrane permeation flux also decreases, so it is preferably above 5°C and below 45°C. In addition, if the pH of the supply water becomes high, in the case of supply water with a high salt concentration such as seawater, scale such as magnesium may be generated. In addition, the composite semipermeable membrane may be degraded due to high pH operation, so it is preferably operated in the neutral region.

[0138] As the raw water treated by the composite semipermeable membrane involved in this embodiment, there can be cited, for example, a liquid mixture of 50 mg / L to 100 g / L of salt (Total Dissolved Solids) such as seawater, salt water, and drainage. Generally speaking, salt refers to the total dissolved solid content, expressed as "mass ÷ volume" or "weight ratio". According to the definition, the solution filtered with a 0.45 μm filter can be evaporated at a temperature of 39.5 to 40.5°C, and the weight of the residue can be calculated, or more simply converted from the practical salinity (S).

[0139] Example

[0140] The present invention is described in more detail below by way of examples, but the present invention is not limited to these examples.

[0141] (Reference Example 1)

[0142] A support membrane was prepared by casting a 18 wt % DMF solution of polysulfone at a thickness of 200 μm on a polyester nonwoven fabric composed of long fibers at room temperature (25° C.), immediately immersing it in pure water, and leaving it for 5 minutes.

[0143] (Example 1)

[0144] The support membrane obtained in Reference Example 1 was immersed in an aqueous solution containing 4 wt% of m-phenylenediamine (m-PDA) for 2 minutes, and the support membrane was slowly lifted in a vertical direction, and nitrogen gas was blown from an air nozzle to remove excess aqueous solution from the surface of the support membrane. Next, a n-decane solution (water content 23 ppm) containing 0.12 wt% of trimesoyl chloride (TMC) was applied as the first polyfunctional acid halide solution.

[0145] Then, within 5 seconds, on the first polyfunctional acid halide solution layer, a n-decane solution (water content 10 ppm) containing 0.12 wt% of trimesoyl chloride (TMC) was further applied as the second polyfunctional acid halide solution in such a manner that the surface of the supporting membrane was completely wetted. Next, the membrane was heated in an oven at 100°C, and then, in order to remove the excess solution from the membrane, the membrane was vertically drained and dried by blowing air at 20°C using a blower. Finally, the membrane was washed with pure water at 90°C, thereby obtaining a composite semipermeable membrane.

[0146] The water content contained in the first and second polyfunctional acid halide solutions is shown in Table 1. The maximum width Wa of the protrusions, the root width Wb of the protrusions, the maximum width Wa of the protrusions / the root width Wb of the protrusions, the average number density of the protrusions, the filling circle diameter, the actual length of the film, the height (existence ratio) of the protrusions, the thickness of the film, and the membrane permeation flux of the separation functional layer surface of the obtained composite semipermeable membrane are shown in Table 2.

[0147] (Examples 2 to 11)

[0148] Except that the water contents in the first and second polyfunctional acid halide solutions were changed to concentrations shown in Table 1, the same operation as in Example 1 was carried out to obtain a composite semipermeable membrane.

[0149] (Examples 12 to 17)

[0150] The composite semipermeable membrane was obtained in the same manner as in Example 1 except that the water content in the first and second polyfunctional acid halide solutions was changed to the concentrations shown in Table 1 and additives were added to the first and second polyfunctional acid halide solutions. The types and concentrations of the additives contained in the first and second polyfunctional acid halide solutions are shown in Table 1.

[0151] (Comparative Examples 1-2)

[0152] A composite semipermeable membrane was obtained in the same manner as in Example 1 except that only the first polyfunctional acid halide solution containing the amount of water shown in Table 1 was applied.

[0153] (Comparative Examples 3 to 4)

[0154] Except having changed the water content contained in the 1st and 2nd polyfunctional acid halide solutions into the concentration shown in Table 1, it carried out similarly to Example 1, and obtained the composite semipermeable membrane.

[0155] (Comparative Example 5)

[0156] The support membrane obtained in Reference Example 1 was immersed in an aqueous solution containing 2.0 wt% m-PDA and 1.5 wt% N-methylpyrrolidone as an additive for 2 minutes, and the support membrane was slowly lifted in a vertical direction, and nitrogen was blown from an air nozzle to remove excess aqueous solution from the surface of the support membrane. Next, as the first and second polyfunctional acid halide solutions, hexane solutions containing 0.05 wt% trimesoyl chloride and 1 wt% ethyl octanoate as an additive were sequentially applied in a manner that the surface of the support membrane was completely wetted. The water content of the first and second polyfunctional acid halide solutions is shown in Table 1.

[0157] Then, in order to remove excess solution from the membrane, the membrane was drained vertically and dried by blowing air at 20° C. using a blower. Finally, the membrane was washed with pure water at 90° C. to obtain a composite semipermeable membrane.

[0158] (Comparative Example 6)

[0159] The support membrane obtained in Reference Example 1 was immersed in 2.0 wt% m-PDA for 2 minutes, and the support membrane was slowly lifted in the vertical direction, and nitrogen was blown from the air nozzle to remove the excess aqueous solution from the surface of the support membrane. Next, the aqueous solution was concentrated at 80°C for 1 minute using a hot air dryer, and then, as the first and second polyfunctional acid halide solutions, a 0.1 wt% n-decane solution of trimesoyl chloride was applied in sequence in such a manner that the surface of the support membrane was completely wetted. The water content of the first and second polyfunctional acid halide solutions is shown in Table 1.

[0160] Then, in order to remove excess solution from the membrane, the membrane was drained vertically and dried by blowing air at 20° C. using a blower. Finally, the membrane was washed with pure water at 90° C. to obtain a composite semipermeable membrane.

[0161] (Measurement of the maximum width of protrusions in the separation functional layer, the root width of protrusions, the diameter of the filling circle, the height of protrusions (existence ratio), the thickness of the film, and the actual length of the film)

[0162] These parameters were measured by the above-mentioned methods. The sample was coated with ruthenium tetroxide, and a Hitachi S-900 electron microscope was used as a high-resolution field emission scanning electron microscope.

[0163] (Method for measuring the average number density of protrusions in the separation functional layer)

[0164] The composite semipermeable membrane sample was embedded with epoxy resin, stained with OsO4 in order to easily observe the cross section, cut it with an ultrathin slicer, and made 10 ultrathin sections. For the obtained ultrathin sections, a cross-sectional photograph was taken using a transmission electron microscope. The accelerating voltage during observation was 100 kV, and the observation magnification was 10,000 times. For the obtained cross-sectional photograph, the number of protrusions on the cross section with a length of 2.0 μm in the membrane surface direction was measured using a scale, and the 10-point average surface roughness was calculated as described above. Based on the 10-point average surface roughness, a portion with a height of more than 1 / 5 of the 10-point average surface roughness was taken as a protrusion, and its number was counted to obtain the average number density of the protrusions of the separation functional layer.

[0165] (Water content in polyfunctional acid halide solution)

[0166] The amount of water contained in the polyfunctional acid halide solution was measured five times in advance using a trace water content measuring device CA-05 manufactured by Mitsubishi Chemical Industries, Ltd., and the average value was determined.

[0167] (Evaluation of membrane performance under low pressure)

[0168] (Membrane flux)

[0169] The composite semipermeable membrane was supplied with raw water (NaCl concentration 3.2%, boron concentration about 5 ppm) adjusted to a temperature of 25°C and a pH of 6.5 at an operating pressure of 4.1 MPa. The membrane filtration treatment was performed for 24 hours. The amount of water permeated through the membrane was expressed as the amount of water permeated (cubic meters) per square meter of membrane surface per day as the membrane permeation flux (m 3 / m 2 / day).

[0170] [Table 1]

[0171] [Table 1]

[0172]

[0173] [Table 2]

[0174] [Table 2]

[0175]

[0176] As can be seen from the results in Table 2, in Examples 1 to 17, the values ​​of the membrane permeation fluxes under the low-pressure operation were larger than those in the comparative examples.

[0177] The present invention is described in detail with reference to specific embodiments, but it is obvious to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent application (Special Application 2021-072382) filed on April 22, 2021, and its contents are cited here as a reference.

[0178] Industrial Applicability

[0179] The composite semipermeable membrane of the present invention is particularly suitable for desalination of seawater and salt water.

Claims

1. A composite semipermeable membrane comprising a supporting membrane and a separation functional layer provided on the supporting membrane, wherein the separation functional layer is a separation functional layer mainly composed of polyamide formed by interfacial polycondensation of a polyfunctional amine and a polyfunctional acyl halide, wherein: The separation function layer has a plurality of protrusions formed of a thin film, In cross sections of any 10 locations with a length of 2.0 μm in the film surface direction of the supporting film, a ratio (Wa / Wb) of a maximum width Wa of the protrusion to a base width Wb of the protrusion of at least a part of the plurality of protrusions is greater than 1.3 and less than 2.0, The separation function layer is formed by a process having the following steps: (i) a step of contacting the support membrane with a polyfunctional amine solution; (ii) after the above step (i), a step of contacting the supporting membrane with a polyfunctional acid halide solution to form polyamide on the supporting membrane by interfacial polycondensation; In step (ii), a layer of the polyfunctional acid halide solution is formed by applying polyfunctional acid halide solutions having different water contents on the supporting membrane multiple times, wherein the layer of the polyfunctional acid halide solution has a gradient in which the water content increases as the layer approaches the supporting membrane.

2. The composite semipermeable membrane according to claim 1, wherein The separation functional layer has protrusions whose maximum diameter R of a circle accommodated inside is 30 nm or more.

3. The composite semipermeable membrane according to claim 1 or 2, wherein The average number density of the protrusions in the separation functional layer is 10 or more / μm and 20 or less / μm.

4. The composite semipermeable membrane according to claim 3, wherein The actual length L of the thin film per 1 μm of the supporting film in the film surface direction of the thin film is 3.0 μm or more, The thickness of the thin film is greater than 15 nm.

5. The composite semipermeable membrane according to claim 4, wherein Among the plurality of protrusions, a ratio of the number of protrusions having a height of 200 nm or more to the number of protrusions having a height of 10 nm or more is 1 / 20 or more and 1 / 2 or less.

6. The composite semipermeable membrane according to claim 4, wherein Among the plurality of protrusions, a ratio of the number of protrusions having a height of 400 nm or more to the number of protrusions having a height of 10 nm or more is 1 / 20 or more and 1 / 5 or less.

7. The composite semipermeable membrane according to claim 5, wherein Among the plurality of protrusions, a ratio of the number of protrusions having a height of 400 nm or more to the number of protrusions having a height of 10 nm or more is 1 / 20 or more and 1 / 5 or less.

Citation Information

Patent Citations

  • Laminated semipermeable membrane and production thereof

    JP1990078428A

  • Production of thin composite film

    JP1994047260A

  • Productionn of high permeable composite reverse osmosis membrane

    JP1996224452A

  • Polyamide-based reverse osmosis separation membrane with excellent initial permeate flow rate and method for producing the same

    JP2014521499A

  • Thermoelectric conversion element and thermoelectric conversion device equipped with the same

    JP2021072382A