Cookware, cooking utensils and cooking method thereof
By forming a spray layer containing titanium, iron and oxygen on the pot, and adding a nitrided layer in the nitriding process, the problem of insufficient acid and salt water corrosion resistance of the pot is solved, and food safety and user experience are improved. .
Patent Information
- Application Number
- CN202310997312.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-08-09
AI Technical Summary
Existing pots are not resistant to acid and salt water corrosion, and stainless steel woks contain high levels of heavy metal elements, which affects food safety, and the poor color of the oxide film of non-stick pots affects user experience.
A melt-sprayed layer with a thickness of 5 μm to 80 μm is used, containing 48% to 55% of titanium, 11% to 15% of iron, and 28% to 35% of oxygen. It is sprayed through a melt spraying process and nitrided The nitrided layer is added in the process to form a pot with higher corrosion resistance and economic benefits, as well as stable color.
Significantly improve the acid and salt water corrosion resistance of the pot, reduce the use of heavy metal elements, improve food safety, and the color is close to traditional iron pots, enhancing user experience.
Smart Images

Figure CN117179570B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cooking utensils, and in particular to a cooker, a method for processing and preparing the cooker, and the cooking utensil. Background Art
[0002] Woks are the most commonly used tools in the kitchen, and iron woks are accepted and recognized by most consumers due to their long service life, rapid and uniform heat conduction, and easy maintenance. However, iron woks have poor acid and salt water corrosion resistance during long-term cooking.
[0003] In order to avoid the acid resistance and corrosion resistance problems of iron woks, stainless steel woks are made on the market by adding various heavy metal elements such as chromium, nickel, molybdenum, etc. to improve the strength and corrosion resistance. However, the corrosion resistance of stainless steel woks is limited, and their heavy metal content is relatively high. Long-term use may cause consumers to ingest some heavy metal elements, which is not conducive to food safety.
[0004] Some corrosion-resistant cookware are provided in the prior art. For example, patent CN114983238A provides a cooking container with a high-temperature creep-resistant metal coating and a manufacturing method thereof. In this technical solution, a spray layer is formed by spraying the surface of the pot body substrate, wherein the spraying raw materials of the spray layer include iron and titanium, and are also doped with chromium, nickel and molybdenum to take into account the wear resistance, corrosion resistance and acid resistance of the non-stick pan. However, this method still uses a large amount of heavy metal elements, which is not conducive to improving food safety.
[0005] In addition, some non-stick pans currently on the market contain titanium in their sprayed layers, which will form a titanium-containing oxide film on the surface. The oxide film will appear colorful, such as yellowish or bluish, which has a low visual acceptance among users and affects the user experience. Summary of the invention
[0006] In order to solve the above problems, the present invention aims to provide a cookware that can have higher food safety and significantly improve corrosion resistance. It can be understood that the corrosion resistance described in the present application includes acid corrosion resistance (such as 2% citric acid solution) and salt water corrosion resistance (such as 5% NaCl salt water).
[0007] On the one hand, the present application provides a cookware, comprising a cookware base and a sprayed layer with a thickness of 5 μm to 80 μm, wherein the sprayed layer covers the inner surface of the cookware base;
[0008] In terms of mass percentage, the sprayed layer includes 48% to 55% of titanium and 11% to 15% of iron, with the remainder being inevitable impurities.
[0009] It can be understood that the sprayed layer is formed by spraying the sprayed raw material through the spraying process. In the spraying process, the metal powder in the sprayed raw material is easily oxidized by oxygen in the air to form oxides, that is, the sprayed layer also contains oxygen element. Preferably, by mass percentage, the oxygen element accounts for 28%~35% of the sprayed layer, that is, the sprayed layer includes 48%~55% of titanium element, 11%~15% of iron element and 28%~35% of oxygen element, and the remainder is unavoidable impurities.
[0010] The cookware having the sprayed layer formed by the above-mentioned element composition, the sprayed raw materials contain titanium material and iron material. Among them, adding part of the iron material to the sprayed raw materials containing titanium material can reduce costs and increase economic benefits on the one hand; on the other hand, the thermal expansion coefficient of the cookware sprayed layer obtained in this way is closer to the cookware substrate using an iron matrix, and thus the adhesion is better, which effectively prevents the sprayed layer from falling off. In addition, the iron element is more likely to generate a nitrogen mixture in the nitriding process, so that the nitrided layer formed on the sprayed layer is thicker, the nitriding effect is better, and it is more conducive to the subsequent further nitriding of the sprayed layer.
[0011] In addition, the color of the oxide film formed by the addition of iron materials will be closer to the black color of traditional iron pans, which will make the color of the pot stable, significantly enhance the user experience, and at the same time show significantly improved corrosion resistance compared to traditional iron pans.
[0012] In one embodiment, the sprayed layer further includes 1.2% to 2% of aluminum element by mass.
[0013] Among them, adding aluminum elements to the spraying raw materials can form aluminum oxide through high-temperature oxidation during spraying. Aluminum oxide has a relatively high hardness, which helps to improve the overall hardness of the spraying layer.
[0014] In one embodiment, the sprayed layer includes, by mass percentage, 49% to 53% of titanium, 12% to 14% of iron, and 1.3% to 1.5% of aluminum, with the remainder being unavoidable impurities.
[0015] It can be understood that the metal of the cookware having the sprayed layer formed by the above-mentioned elemental composition also exists in the form of oxide in the sprayed layer. At this time, the mass proportion of oxygen in the sprayed layer is preferably 29%~34%, that is, the preferred elemental composition of the sprayed layer in the present application is: 49%~53% titanium, 12%~14% iron, 1.3%~1.5% aluminum, and 29%~34% oxygen.
[0016] In one embodiment, a nitride layer is formed on the inner surface of the cookware substrate, the nitride layer at least partially covers the sprayed layer, and the thickness of the nitride layer is 10 μm to 20 μm.
[0017] Preferably, the thickness of the sprayed layer is 20-80 μm, more preferably 20-50 μm.
[0018] Preferably, the surface of the sprayed layer away from the cookware substrate before the nitriding process has a concave-convex structure, such as a concave-convex surface formed by adjacent convex structures and concave structures. When the sprayed layer is nitrided, the total area of the concave-convex surface is larger than the total area of the planar structure, so the contact area with the nitriding gas is larger, which is more conducive to the nitriding gas infiltrating the sprayed layer to react to form a nitriding layer, and finally makes the average thickness of the nitriding layer thicker, thereby improving the protective effect of the nitriding layer on the cookware substrate, especially the salt resistance.
[0019] Preferably, the concavo-convex structure can make the surface roughness of the inner surface of the final cookware product Ra 1.5 μm-3.0 μm after further processing, and the further processing includes but is not limited to polishing.
[0020] In addition, since the sprayed layer contains a relatively high proportion of titanium material, which has good acid and alkali resistance, it helps to improve the acid and alkali resistance of the cookware; the nitride layer located on the surface of the sprayed layer has good salt resistance, which helps to improve the corrosion resistance of the cookware. At the same time, the nitride layer also has good hardness, which improves the wear resistance of the cookware.
[0021] In addition, since the sprayed layer also contains iron material, the iron material will generate iron oxide after high temperature and nitridation. The iron oxide is black, making the color of the pot surface similar to that of an iron pot, thereby improving user acceptance.
[0022] In one embodiment, the material of the cookware base is selected from at least one of cast iron, cold-rolled steel, iron alloy, aluminum, aluminum alloy, copper and copper alloy.
[0023] Preferably, the material of the cookware base is selected from cast iron or cold-rolled steel.
[0024] On the other hand, the present application also provides a method for processing and preparing the above-mentioned cookware, comprising the steps of sequentially performing primary polishing, sandblasting, thermal spraying, nitriding, and secondary polishing on the cookware substrate;
[0025] Wherein, the sprayed layer is formed on the inner surface of the cookware base through the spraying step.
[0026] In one embodiment, the spraying is performed by one of thermal spraying, plasma spraying and / or cold spraying; and / or,
[0027] Calculated by mass percentage, the raw materials used for the thermal spraying include 65% to 75% titanium material and 18% to 25% iron material, and the remainder is inevitable impurities.
[0028] Optionally, an embodiment of the processing and preparation method includes the following steps: forming the substrate into a pot body having an inner cavity; polishing the surface of the pot body facing the inner cavity; sandblasting the surface of the inner cavity to form a rough surface; spraying the spray material on the surface of the inner cavity to form the spray layer on the rough surface; performing a first nitriding treatment on the pot body to form a pre-nitriding layer on the spray layer; polishing the pot body having the spray layer and the pre-nitriding layer; performing a second nitriding treatment on the polished pot body to form a nitriding layer based on the pre-nitriding layer.
[0029] In these embodiments, the cookware is subjected to secondary nitriding. On the one hand, the total nitriding time is increased, which helps nitrogen to penetrate deeper into the sprayed layer, thereby increasing the total thickness of the nitrided layer; on the other hand, polishing is performed between the two nitridings to remove impurities remaining on the surface of the cookware during the first nitriding, so that nitrogen can more easily penetrate into the nitrided layer formed by the first nitriding during the second nitriding, which helps to make the nitrided layer denser, thereby forming a dense nitrided layer with a high nitrogen content. It can be seen that these embodiments can form a dense nitrided layer, so that the cookware has better corrosion resistance.
[0030] Optionally, as an alternative to the above-mentioned embodiment, an embodiment of the processing and preparation method includes the following steps: forming the substrate into a pot body having an inner cavity; polishing the surface of the pot body facing the inner cavity; sandblasting the surface of the inner cavity to form a rough surface; nitriding the pot body to form a nitride layer of the pot body on the rough surface; spraying a spray material on the surface of the nitride layer of the pot body to deposit the spray layer on the surface of the nitride layer of the pot body; and nitriding the pot body for a second time to form the nitride layer on the spray layer.
[0031] In these embodiments, during the first nitriding, nitrogen penetrates into the pot body from the surface of the pot body. During this process, since the pot body contains less nitrogen, the pot body is easy to react with nitrogen to generate corresponding nitrides, and the nitriding rate is fast, so that a pot body nitride layer that meets the requirements can be formed quickly. In addition, the pot body is generally made of materials such as cast iron, cold-rolled steel plate and iron alloy. Iron elements are more likely to generate nitrogen mixtures during the nitriding process, so that the nitriding layer formed on the sprayed layer is thicker and the nitriding effect is better. Similarly, during the second nitriding, nitrogen penetrates into the sprayed layer from the surface of the sprayed layer. Since the nitrogen content of the sprayed layer is less, the sprayed layer is easy to react with nitrogen to generate corresponding nitrides, and the nitriding rate is fast, so that the nitriding layer can be formed quickly.
[0032] Optionally, the nitride layer is completely contained in the sprayed layer, the hardness of the nitride layer is greater than the hardness of the pot body, and the hardness of the pot body is greater than the hardness of the sprayed layer.
[0033] In these embodiments, the hardness of the unnitrided portion of the melt-sprayed layer is relatively low, so the unnitrided portion of the melt-sprayed layer has better toughness than the pot body. In daily use, the pot is often heated and cooled, so the pot body, the melt-sprayed layer and the nitride layer expand and contract repeatedly, and the thermal expansion coefficients of the pot body and the melt-sprayed layer are different, so the deformation of the pot body and the melt-sprayed layer is different during the expansion and contraction process, so that the pot body and the melt-sprayed layer will generate interaction forces based on the difference in deformation. Since the toughness of the melt-sprayed layer is better than that of the pot body, the energy generated by the above-mentioned interaction force can be partially absorbed by the melt-sprayed layer based on its own toughness, which helps to reduce the possibility of fracture problems, and in a certain sense, it can make the pot body and the melt-sprayed layer have a reliable connection firmness. The nitride layer is located on the surface of the inner cavity and has a greater hardness than the pot body and the melt-sprayed layer, so that the surface of the inner cavity still has good wear resistance.
[0034] Preferably, the spraying raw material is in powder form with a particle size of 170 μm to 300 μm. Within this particle size range, the spraying effect can be ensured while avoiding combustion.
[0035] The nitriding step adopts thermal nitriding, and the heating temperature of the thermal nitriding is 500-600°C.
[0036] Optionally, the first polishing and second polishing steps may adopt the following process: use a scouring pad, sandpaper, mechanical polishing equipment or chemical method to grind and polish the inner surface of the cookware base to remove oil stains and impurities on the surface of the cookware base.
[0037] Optionally, the sandblasting step may adopt the following process: using a high-speed sand stream to impact the surface of the cookware substrate so that the roughness of the cookware substrate is Ra 2.0 μm ~ Ra 10 μm;
[0038] Optionally, the method further comprises the steps of cleaning and oiling after the secondary polishing.
[0039] In one embodiment, the titanium material is selected from one or more of metallic titanium, titanium oxide or titanium alloy; and / or,
[0040] The iron material is selected from one or more of metallic iron, iron oxide or iron alloy.
[0041] In one embodiment, the spraying raw material further includes 2% to 8% of aluminum material, and the aluminum material is selected from one or more of metallic aluminum, aluminum oxide or aluminum alloy.
[0042] In a preferred embodiment, the titanium material, the iron material and the aluminum material are respectively metal titanium, metal iron and metal aluminum.
[0043] It should be noted that the "impurities" described in this application may come from the spraying raw materials, such as S, P, Si, Mn and other elements in iron materials, or C, H, Mg and other elements in titanium materials. When there are other spraying raw materials (such as aluminum materials), other impurities will also be introduced.
[0044] On the other hand, the present application also provides a cooking utensil, including the above-mentioned pot; wherein the cooking utensil includes one of a frying pan, an electric rice cooker, an electric pressure cooker, a soymilk maker, and a food processor.
[0045] Preferably, the cooking utensil is a frying pan.
[0046] This application has at least the following beneficial effects:
[0047] 1. The cookware provided by the present application has a sprayed layer in which a portion of iron material is added to the sprayed raw material containing titanium material, which can reduce costs and increase economic benefits. At the same time, the thermal expansion coefficient of the sprayed layer of the cookware obtained in this way is closer to the cookware substrate using an iron matrix, and thus the adhesion is better, which effectively prevents the sprayed layer from falling off. In addition, the iron element is more likely to generate a nitrogen mixture in the nitriding process, so that the nitrided layer formed on the sprayed layer is thicker, the nitriding effect is better, and it is more conducive to the subsequent need for further nitriding of the sprayed layer. Moreover, the color of the oxide film formed by the addition of iron material will be closer to the black color of the traditional iron pan, thereby making the color of the cookware stable, significantly enhancing the user experience, and at the same time being able to show significantly improved corrosion resistance compared to the traditional iron pan.
[0048] 2. The processing and preparation method of the cookware provided in this application is simple to operate and easy to apply in actual production processes. The inner wall of the obtained cookware does not contain heavy metal elements, which is more conducive to food safety and improves the user experience. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0050] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0051] In the attached picture:
[0052] Figure 1 It is a structural schematic diagram of an implementation mode of the cookware provided by the present application;
[0053] Figure 2 yes Figure 1Enlarged view of part A in the middle;
[0054] Figure 3 This is a real picture of the cookware prepared in Example 2 of Example 3;
[0055] Figure 4 This is a real picture of a cookware made of pure titanium metal.
[0056] In the figure:
[0057] 1. Cookware substrate; 2. Spraying layer; 3. Nitriding layer; 301. Protruding structure; 302. Concave structure. DETAILED DESCRIPTION
[0058] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below in an exemplary manner in conjunction with the accompanying drawings.
[0059] It should be noted that many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0060] In addition, in the description of the present application, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0061] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0062] In the present application, unless otherwise clearly specified and limited, a first feature "above" or "below" a second feature may be that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in an appropriate manner in any one or more embodiments or examples.
[0063] Unless otherwise specified, in the following embodiments, the reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.
[0064] If no specific conditions are specified in the examples, the experiments were carried out according to conventional conditions or conditions recommended by the manufacturer.
[0065] Example 1 Processing and preparation method of cookware
[0066] This embodiment provides a method for processing and preparing a cookware, comprising the following steps:
[0067] Step 1) Polishing: Use a scouring pad or sandpaper to polish the inner surface of the cookware base to remove oil and impurities on the surface of the cookware base.
[0068] Step 2), sand blasting: use high-speed sand flow to impact the surface of the cookware base to make the roughness of the cookware base Ra2.0μm ~10μm;
[0069] Step 3), spraying: Mix the spraying raw material powder with a particle size of 170μm~300μm and pass it into the spraying gun, and thermally spray the mixed powder on the inner wall of the cookware substrate at a power of about 40kw. After cooling, the liquid spraying raw material mixture condenses on the inner surface of the nitride layer of the cookware substrate to form a spraying layer;
[0070] Step 4), nitriding: placing the cookware substrate after the spraying in a nitriding furnace, introducing ammonia and carbon dioxide in a ratio of 16-20:0.5-4 into the nitriding furnace for nitriding treatment, the temperature is 500°C-600°C, the time is about 7 hours, so as to form a nitrided layer with a thickness of 10000 mm on the inner wall surface of the cookware substrate;
[0071] Step 5) Secondary polishing: Use a scouring pad or sandpaper to polish the inner surface of the nitride layer to make the surface roughness of the nitride layer Ra 1.5μm~Ra 3.0μm.
[0072] Step 6), clean and oil.
[0073] Example 2 Cookware.
[0074] This embodiment provides a cookware obtained by the processing and preparation method provided in Example 1. The structure of the cookware is as follows: Figure 1-2 The pot prepared in the above embodiment can be a frying pan, or an inner pot of a cooking appliance such as an electric rice cooker, an electric pressure cooker, a soybean milk maker, a food processor, etc., preferably a frying pan.
[0075] In such Figure 1 In the embodiment shown, the pot is a frying pan, and the pot body thereof comprises a pot base 1, a sprayed layer 2 and a nitride layer 3 from the bottom to the top.
[0076] Among them, the pot substrate 1 can be made of any one of cast iron, cold-rolled steel plate, iron alloy, aluminum, aluminum alloy, copper and copper alloy, preferably cast iron or cold-rolled steel plate. The sprayed layer 2 is connected to the pot substrate 1 and at least partially covers the pot substrate 1, preferably completely covers the pot substrate 1, and the sprayed raw material is sprayed on the inner surface of the pot substrate 1 by thermal spraying, ion spraying or cold spraying through a spraying process, with a thickness of 1-100μm, preferably 5-80μm. The nitride layer 3 is connected to the sprayed layer 2 and at least partially covers the sprayed layer 2, preferably completely covers the inner surface of the sprayed layer 2. In a preferred embodiment, the nitride layer 3 is formed by a nitriding process on the inner surface of the sprayed layer 2, with a thickness of 10-20μm.
[0077] See also Figure 2 The inner surface of the nitride layer 3 away from the cookware base 1 has a concavo-convex structure, for example, a concavo-convex surface 302 formed by adjacent convex structures 301 and concave structures. The nitride layer 3 with such a structure is formed by spraying a spray material on the uneven inner surface of the cookware base 1 formed by sandblasting to form a spray layer with the same concavo-convex structure through a spray process, and then nitriding the spray layer. When the spray layer 2 with a concavo-convex structure is nitrided, the total area of the concavo-convex surface is larger than the total area of the planar structure, so the contact area with the nitriding gas (such as ammonia) is larger, which is more conducive to the nitriding gas infiltrating the spray layer to react and form the nitride layer 3, and finally the average thickness of the nitride layer 3 is thicker, thereby improving the protective effect of the nitride layer 3 on the cookware base 1, especially the salt resistance.
[0078] After the second polishing, the surface roughness of the nitride layer 3 is Ra 1.5μm~Ra 3.0μm, that is, the surface of the nitride layer 3 is a relatively smooth surface, which can help reduce the sticking of ingredients and the spatula and the pot when cooking and stir-frying, improve the hand feel, and make the inner surface of the pot present a smooth and beautiful appearance.
[0079] It should be noted that, since the nitride layer 3 also has a certain thickness, the secondary polishing mainly polishes the surface of the nitride layer 3. Since the nitride layer 3 has good hardness, the nitride layer 3 can form a physical protection for the sprayed layer 2, which helps to reduce the probability of accidentally damaging the sprayed layer 2 during the secondary polishing operation.
[0080] In addition, the sprayed layer 2 and the nitrided layer 3 contain iron materials. After spraying and nitriding, the iron materials contain a large amount of iron oxide. The chemical properties of iron oxide are relatively stable, so it can provide a certain degree of protection for the cookware. In addition, iron oxide is black, so that the surface of the cookware can be as Figure 3 The black color shown here is slightly yellow compared to the iron-free titanium pan (such as Figure 4 The color of the pan (as shown) is closer to that of a pure iron pan, which helps improve user acceptance.
[0081] Example 3 Corrosion resistance test of cookware made of different spraying materials
[0082] This embodiment adopts the processing and preparation method provided in Embodiment 1, and adopts the melt-sprayed raw material composed of metal titanium, metal iron and metal aluminum (wherein the total mass of metal titanium, metal iron and metal aluminum is 100%, and the element composition of the mixed melt-sprayed raw material after mixing is 70% Ti + 21% Fe + 5% Al + 4% impurities) to process and manufacture cookware, and takes the cookware without spraying layer, that is, the commonly used iron pot without spraying layer as a comparative example, and tests the impact resistance, acid resistance and salt water corrosion resistance of each example.
[0083] Among them, the impact resistance test method is as follows:
[0084] Take a small iron ball of about 230g, select several positions on the surface of the cookware, and drop the small iron ball from a height of 1.5m to the selected positions to impact the surface of the cookware. Repeat this process 5 times and observe the surface conditions of the impacted positions.
[0085] The test method for acid resistance is as follows:
[0086] Pour a solution containing about 2% citric acid into the pot and let it sit, then observe the shedding condition on the surface of the pot.
[0087] The test method for salt water corrosion resistance is as follows:
[0088] Pour a 5% salt solution into the pot and boil it, then observe the corrosion on the pot surface while the solution is still slightly boiling. Slightly boiling means that the solution has boiled but not violently.
[0089] The results are shown in Table 1:
[0090] Table 1
[0091] Example Melt spraying raw materials Spraying layer thickness Impact resistance test 5% salt water corrosion resistance test 2% citric acid resistance test D1 - - - Corrosion spots appear in 20 minutes Surface peeling in 1 hour D2 65%Ti+26%Fe+5%Al+4%Impurities 21-50μm After 5 experiments, no fusion layer fell off. A small amount of corrosion spots appeared within 1 hour Part of the surface fell off after 15 hours 1 70%Ti+21%Fe+5%Al+4%Impurities 5-20μm After 5 experiments, no fusion layer fell off. No abnormality for 20 minutes 11 hours without abnormality 2 70%Ti+21%Fe+5%Al+4%Impurities 21-50μm After 5 experiments, no fusion layer fell off. 1.5 hours without abnormality No abnormality in 24 hours 3 70%Ti+21%Fe+5%Al+4%Impurities 51-80μm After 2 experiments, the sprayed layer fell off. 1.5 hours without abnormality 39 hours without abnormality 4 70%Ti+21%Fe+5%Al+4%Impurities More than 80μm After one experiment, the sprayed layer fell off. 1.5 hours without abnormality 45 hours without abnormality
[0092] From the results in Table 1, it can be seen that when the thickness of the sprayed layer is greater than 80 μm, the impact resistance of the sprayed layer is significantly reduced, that is, the adhesion between the sprayed layer and the cookware substrate is significantly reduced, and the risk of the sprayed layer falling off is high, which reduces the life of the cookware. At the same time, the cookware prepared by the processing and preparation method provided in this application has significantly improved corrosion resistance.
[0093] Moreover, the Ti content in the sprayed layer has a certain influence on the acid resistance of the cookware. Specifically, it can be seen from the data of Example 2 and Example D2 in Table 1 that when the Ti content is 65%, the sprayed layer partially falls off in 2% citric acid in 15 hours, which is a significant decrease compared to the 24 hours without abnormality in Example 2. The acid resistance is almost close to that of Example 1. It can be inferred that further reducing the Ti content may lead to the acid resistance of the sprayed layer and its unsatisfactory performance. When the Ti content reaches 70%, it shows better acid resistance at all thicknesses. However, when the Ti content is higher than 75%, the manufacturing cost of the cookware will increase. Therefore, the sprayed raw material of the present application can optionally include 65% to 75% of titanium material, so as to provide a better market prospect with high cost performance while improving the excellent corrosion resistance of the cookware.
[0094] Taking the cookware made in Example 2 as an example, the element composition of the sprayed layer in the three batches of cookware products made therein is as follows:
[0095] Product 1: Ti 49.5%, Fe 13.3%, O 33.7%, Al 1.3%, the remainder is impurities;
[0096] Product 2: Ti 54.1%, Fe 14.2%, O 29.2%, Al 1.5%, the remainder is impurities;
[0097] Product three: Ti 50.3%, Fe 13.8%, O 31.3%, Al 1.3%, and the balance is impurities.
[0098] It can be seen from this that the cookware obtained by using the sprayed raw materials provided in the embodiments of the present application and the processing and preparation method of the present application has a composition of the sprayed layer within a reasonable error range between batches.
[0099] It should be noted that, in the embodiment in which the thickness of the sprayed layer is less than 20 μm, although the corrosion resistance is reduced compared with the embodiment in which the thickness of the sprayed layer is greater than 20 μm, the corrosion resistance of the embodiment is still better than that of the iron pot without the sprayed layer, and the purpose of the invention can be achieved; and the impact resistance of the embodiment in which the thickness of the sprayed layer is greater than 50 μm is also reduced compared with the embodiment in which the thickness of the sprayed layer is less than 50 μm, but the decline is not obvious, and it still has certain practical value compared with the embodiment in which the thickness of the sprayed layer is greater than 80 μm, so these embodiments are also within the scope of protection of this application.
[0100] In the meantime, see Figure 3 and Figure 4 .in Figure 4 This is a real picture of a cookware whose sprayed raw material is pure metallic titanium. It can be seen from the picture that the surface of the sprayed layer is beige. Figure 3 This is a picture of the actual cookware prepared in Example 2. It can be seen from the picture that the surface of the sprayed layer is black, which is close to the cast iron cookware base, and is more in line with the usage experience of most users in the market.
[0101] Example 4 Processing and preparation method of cookware
[0102] This embodiment provides a method for processing and preparing a cookware, comprising the following steps:
[0103] Step 1) Polishing: Use a scouring pad, sandpaper, mechanical polishing equipment or chemical methods to polish the inner surface of the cookware base to remove oil and impurities on the surface of the cookware base.
[0104] Step 2), sand blasting: Use high-speed sand flow to impact the surface of the cookware base to make the roughness of the cookware base Ra2.0μm ~10μm.
[0105] Step 3), spraying: mix the spraying raw material powder with a particle size of 170μm~300μm and pass it into the spraying gun, and thermally spray the mixed powder on the inner wall of the cookware substrate at a power of about 40kw. After cooling, the liquid spraying raw material mixture condenses on the inner surface of the nitride layer of the cookware substrate to form a spraying layer; the spraying raw materials include 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75% titanium material; 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% iron material; 2%, 3%, 4%, 5%, 6%, 7%, 8% aluminum material.
[0106] Step 4), primary nitriding: Place the cookware substrate after spraying in a nitriding furnace, introduce ammonia and carbon dioxide in a ratio of 16~20:0.5~4 into the nitriding furnace for nitriding treatment at a temperature of 500℃~600℃ for about 7 hours to form a pre-nitriding layer on the inner wall surface of the cookware substrate.
[0107] Step 5), secondary polishing: polish the surface of the pre-nitrided layer to remove impurities on the surface of the pre-nitrided layer.
[0108] Step 6), secondary nitriding: placing the cookware substrate after the primary nitriding in a nitriding furnace for secondary nitriding to form a nitrided layer.
[0109] Step 7), three times polishing: Use a scouring pad or sandpaper to polish the inner surface of the nitride layer to make the surface roughness of the nitride layer Ra1.5μm~Ra3.0μm.
[0110] Step 8), clean and oil.
[0111] The nitride layer finally formed in Example 4 is thicker and denser than that in Example 1, and thus has better wear resistance and corrosion resistance.
[0112] In some embodiments, the hardness of the nitride layer is greater than the hardness of the cookware substrate, and the hardness of the cookware substrate is greater than the hardness of the sprayed layer.
[0113] The hardness of the sprayed layer refers to the hardness of the unnitrided portion of the sprayed layer.
[0114] By providing a relatively low hardness sprayed layer, it helps to ensure the firmness of the connection between the sprayed layer and the cookware base; by providing a relatively high hardness nitride layer, the surface of the inner cavity can have better wear resistance.
[0115] Example 5 Processing and preparation method of cookware
[0116] This embodiment provides a method for processing and preparing a cookware, comprising the following steps:
[0117] Step 1) Polishing: Use a scouring pad, sandpaper, mechanical polishing equipment or chemical methods to polish the inner surface of the cookware base to remove oil and impurities on the surface of the cookware base.
[0118] Step 2), sand blasting: Use high-speed sand flow to impact the surface of the cookware base to make the roughness of the cookware base Ra2.0μm ~10μm.
[0119] Step 3), primary nitriding: Place the cookware substrate after spraying in a nitriding furnace, introduce ammonia and carbon dioxide in a ratio of 16~20:0.5~4 into the nitriding furnace for nitriding treatment at a temperature of 500℃~600℃ for about 7 hours to form a nitrided layer on the inner wall surface of the cookware substrate.
[0120] Step 4), spraying: mix the spraying raw material powder with a particle size of 170μm~300μm and pass it into the spraying gun, and thermally spray the mixed powder on the inner wall of the cookware substrate at a power of about 40kw. After cooling, the liquid spraying raw material mixture condenses on the inner surface of the nitride layer of the cookware substrate to form a spraying layer; the spraying raw materials include 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75% titanium material; 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% iron material; 2%, 3%, 4%, 5%, 6%, 7%, 8% aluminum material.
[0121] Step 5), secondary nitriding: placing the cookware substrate after the spraying in a nitriding furnace for secondary nitriding to form a nitrided layer.
[0122] Step 6) Secondary polishing: Use a scouring pad or sandpaper to polish the inner surface of the nitride layer to make the surface roughness of the nitride layer Ra1.5μm~Ra3.0μm.
[0123] Step 7), clean and oil.
[0124] Compared with Example 1, Example 5 has an additional nitriding layer on the pot body, so the resulting pot has better wear resistance and corrosion resistance.
[0125] In some embodiments, the hardness of the pot body nitride layer and the nitride layer is greater than the hardness of the pot substrate, and the hardness of the pot substrate is greater than the hardness of the sprayed layer.
[0126] The hardness of the sprayed layer refers to the hardness of the unnitrided portion of the sprayed layer, that is, the portion of the sprayed layer excluding the nitrided layer.
[0127] By providing a relatively low hardness sprayed layer, it helps to ensure the firmness of the connection between the sprayed layer and the cookware base; by providing a relatively high hardness nitride layer, the surface of the inner cavity can have better wear resistance.
[0128] Example 6 Cookware
[0129] Example 6 is based on Example 2, in which the sprayed layer has a plurality of first micropores, the nitride layer has a plurality of second micropores, and the average pore size of the second micropores in the nitride layer is smaller than the average pore size of the first micropores in the sprayed layer.
[0130] It can be understood that after the thermal spraying and nitriding, the formed thermal spraying layer and the nitrided layer both have a number of micropores of different sizes. The average pore size of the second micropores is smaller than the average pore size of the first micropores, which can also be understood as the nitrided layer being denser than the thermal spraying layer. The second nitriding performed in the embodiment of the above-mentioned pot manufacturing method can make the nitrided layer denser.
[0131] Since the surface of the nitride layer is in direct contact with food, when the average pore size of the second micropores is small, the second micropores can limit the penetration of liquid from the nitride layer into the sprayed layer, so that the nitride layer provides a better protection effect for the sprayed layer. In addition, since the average pore size of the second micropores is small and the second nitride layer is in direct contact with food, the total amount of food penetrating into the second micropores can be reduced, thereby reducing the probability of sticking to the pan.
[0132] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A cookware, characterized in that: It comprises a cookware base body and a sprayed layer with a thickness of 5 μm to 80 μm, wherein the sprayed layer covers the inner surface of the cookware base body; In terms of mass percentage, the sprayed layer includes 48% to 55% of titanium, 11% to 15% of iron and 28% to 35% of oxygen, with the remainder being unavoidable impurities; A nitride layer is formed on the surface of the sprayed layer, the nitride layer at least partially covers the sprayed layer, and the thickness of the nitride layer is 10 μm to 20 μm; The color of the inner surface of the cookware is close to black; The sprayed layer has a plurality of first micropores, the nitride layer has a plurality of second micropores, and the average pore size of the second micropores in the nitride layer is smaller than the average pore size of the first micropores in the sprayed layer.
2. The cookware according to claim 1, characterized in that: In terms of mass percentage, the sprayed layer also includes 1.2% to 2% of aluminum element.
3. The cookware according to claim 2, characterized in that: In terms of mass percentage, the sprayed layer includes 49% to 53% of titanium, 12% to 14% of iron, 1.3% to 1.5% of aluminum, and 29% to 34% of oxygen, with the remainder being unavoidable impurities.
4. The cookware according to claim 1, characterized in that: The material of the cookware base is selected from at least one of cast iron, cold-rolled steel, iron alloy, aluminum, aluminum alloy, copper and copper alloy.
5. A method for preparing a cookware, characterized in that: Used for processing the cookware as claimed in any one of claims 1 to 4; the processing and preparation method of the cookware comprises the steps of sequentially performing a first polishing, sandblasting, thermal spraying, nitriding and a second polishing on the cookware substrate; Wherein, the spraying layer is formed on the inner surface of the cookware base through the spraying step.
6. The method for preparing a cookware according to claim 5, characterized in that: The spraying is performed by one of thermal spraying, plasma spraying and / or cold spraying; and / or, Calculated by mass percentage, the raw materials used for the thermal spraying include 65% to 75% titanium material and 18% to 25% iron material, and the remainder is inevitable impurities.
7. The method for preparing a cookware according to claim 6, characterized in that: The titanium material is selected from one or more of metallic titanium, titanium oxide or titanium alloy; and / or, The iron material is selected from one or more of metallic iron, iron oxide or iron alloy.
8. The method for preparing a cookware according to claim 6, characterized in that: The spraying raw material also includes 2% to 8% of aluminum material, and the aluminum material is selected from one or more of metallic aluminum, aluminum oxide or aluminum alloy.
9. A cooking utensil, characterized in that: It includes the cooker as described in any one of claims 1 to 4; wherein the cooking utensil includes one of a frying pan, an electric rice cooker, an electric pressure cooker, a soymilk maker, and a food processor.
Citation Information
Patent Citations
Cooking container with high-temperature-creep-resistant metal coating and manufacturing method of cooking container
CN114983238A
Wear-resistant coating non-stick pan
CN102835891A
Cookware with high wear resistance and manufacturing method of cookware
CN105476490A
Composite iron non-stick pan and machining process thereof
CN107149388A
Cast iron roasting pot adopting plasma sprayed titanium or titanium alloy
CN108095565A