An integrated multifunctional solar evaporator and a preparation method thereof
By using vertically oriented hydrophilic aerogels and hydrophobic photothermal films in solar evaporators, the problems of low evaporation rate and insufficient salt resistance in the existing technology are solved, and efficient water evaporation and electricity generation are achieved. It has good stability and economy.
Patent Information
- Application Number
- CN202311179417.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-09-13
AI Technical Summary
Existing solar evaporators have a difficult balance between increasing water evaporation rate and salt tolerance, resulting in low and unstable evaporation rate, which limits freshwater production and power generation performance.
Hydrophilic aerogel with a vertically oriented structure is used as the water evaporation layer, combined with a hydrophobic photothermal film and a thermal insulation layer, and is prepared through ice template and freeze-drying methods to achieve rapid transportation and efficient evaporation of water while utilizing photothermal conversion. Efficient hydrophobic membrane transfers heat, increasing evaporation rate and salt tolerance.
Achieving high evaporation rate (6.96kg m-2h-1) and good salt tolerance, it can work continuously in high-salinity seawater for 7 days, meeting the needs of freshwater production and power generation, while having good stability and low-cost preparation .
Smart Images

Figure CN117209000B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an integrated multifunctional solar evaporator for better achieving the balance of water transportation, salt resistance and heat supply and a preparation thereof, belonging to the technical field of functional materials. Background Art
[0002] With the rapid growth of population and the rapid development of economic and industrial globalization, the shortage of fresh water resources has become a common problem faced by the world's human beings. Within the framework of the economic and ecological construction of the dual carbon concept, solar-driven seawater desalination has been regarded as a new technology to solve water shortages and energy needs.
[0003] The water evaporation rate, as one of the key factors in the evaporation water flux of solar-driven desalination, determines the water production and whether it can be used in a practical environment. At present, researchers usually combine these photothermal materials with supporting materials to prepare solar water evaporation devices, such as photothermal films, porous aerogels and hydrogels. At the same time, some artificial transpiration structures, double-layer structures and three-dimensional structures have also been carefully designed to enhance the evaporation rate of water. In addition, technologies such as introducing additional airflow or solar cells into the evaporator and utilizing the solar-electric-thermal effect have also been used to increase the evaporation rate of water. However, the preparation of most solar evaporators is complicated, and the increase in evaporation rate is limited (water evaporation rate <5kg m -2 h -1 (1 sun)), studies on water transport, heat localization, and salt tolerance report a trade-off between high evaporation rates and good salt tolerance.
[0004] On the other hand, thermoelectric conversion modules, salinity gradients, and friction modules are also integrated into solar evaporators to generate electricity. However, in these clean hydropower systems that generate electricity simultaneously, their multifunctional devices are usually non-integrated and require additional components, thereby reducing the evaporation performance of water. In addition, the composite packaging of multiple components in the evaporation system may bring chemical leakage and long-term stability problems.
[0005] In contrast, solar thermal evaporation systems have greater prospects and advantages when evaporating high-concentration brine or real seawater, where the directional flow of ions driven by sunlight produces continuous electrical energy with little impact on evaporation performance. However, the evaporation rate of most (if not all) dual-function evaporators is relatively low (<4kgm -2 h -1 (1 sun). Low evaporation rates not only hinder fresh water production, but also limit the flow of salt ions, thereby limiting power generation.
[0006] Currently, there is no report on an integrated solar evaporator that has both rapid water transportation and stable heating, high evaporation rate and good salt tolerance, while maximizing power generation. Summary of the invention
[0007] The purpose of the present invention is to propose an integrated solar evaporator and a preparation method thereof for better achieving a balance among water transport, salt resistance and heat supply. The comprehensive performance of the prepared solar evaporator, such as water evaporation performance and salt resistance, is greatly improved compared with ordinary evaporators.
[0008] The technical solution of the present invention:
[0009] The first technical problem to be solved by the present invention is to provide an integrated multifunctional solar evaporator, which includes a water evaporation layer, a heating layer and a heat insulation layer. The water evaporation layer is a hydrophilic aerogel with a vertically oriented structure, and the heating layer is a photothermal hydrophobic film.
[0010] Furthermore, in the integrated solar evaporator, the water evaporation layer continuously penetrates the heating layer and the heat insulation layer.
[0011] Furthermore, the hydrophilic aerogel refers to a hydrophilic aerogel with a vertically oriented structure made of a hydrophilic polymer as a matrix and a light-absorbing material as a filler. Hydrophilic aerogels can capture a wide spectrum of solar energy well due to their ultra-high porosity, low density, and high specific surface area, and have broad application prospects in the field of solar-driven water vapor generation; the vertically oriented structure can bring excellent mechanical properties and can also achieve rapid water transportation.
[0012] Furthermore, the content of the light-absorbing filler in the hydrophilic aerogel is 10 to 70 wt%.
[0013] Furthermore, the hydrophilic aerogel is a hydrophilic aerogel with a vertically oriented three-dimensional porous structure, which is prepared by using a hydrophilic polymer and a light-absorbing material as raw materials and adopting an ice template and freeze-drying method.
[0014] Further, the hydrophilic polymer includes at least one of polyvinyl alcohol, polyethylene glycol, polyacrylic acid, sodium polyacrylate, sodium polystyrene sulfonate, polyacrylamide, polyvinylamide or polyethyleneimine, but is not limited thereto. When two polymers are selected, the mass ratio of the first phase to the second phase is 1:2 to 1:9.
[0015] Furthermore, the light-absorbing material can be at least one of metals or metal oxides such as copper, silver, and gold, semiconductors such as titanium trioxide, molybdenum disulfide, and copper sulfide, and carbon materials such as polydopamine, graphite, activated carbon, carbon black, carbon nanotubes, graphene, graphene oxide, and two-dimensional transition metal carbides; but is not limited thereto.
[0016] Furthermore, the hydrophilic aerogel is prepared by the following method: firstly, a hydrophilic polymer solution and a light absorbing material are uniformly mixed to obtain a precursor solution; then, the precursor solution is subjected to an ice template and freeze-dried to obtain a hydrophilic aerogel having a vertically oriented structure;
[0017] Specifically, the hydrophilic aerogel is prepared by the following method: first, a hydrophilic polymer is prepared into a hydrophilic polymer solution; then, a light-absorbing material is ultrasonically dispersed in the hydrophilic polymer solution and mixed to obtain a precursor solution; then, the precursor solution is poured into a mold with polytetrafluoroethylene on the sides and copper on the bottom, and an ice template directional preparation process is used to freeze the mixed solution in the mold (such as contacting the bottom of the mold with a liquid nitrogen bath until the precursor solution is completely frozen); and then, a composite hydrophilic aerogel with a vertically oriented structure is obtained through vacuum freeze drying.
[0018] Furthermore, in the above preparation method, the concentration of the hydrophilic polymer solution is 20-50 mg / ml.
[0019] Furthermore, in the above preparation method, during the freeze-molding process, the freezing temperature is -196 to -78°C, and the freezing time is 180 min to 300 min.
[0020] Furthermore, in the above preparation method, the vacuum freeze-drying time is 48 to 72 hours.
[0021] Furthermore, the photothermal hydrophobic film is prepared by the following method: coating a light-absorbing filler on a base material, immersing the base material in a solution containing a low surface energy hydrophobic polymer material and a curing agent after drying, and finally curing the base material to obtain the photothermal hydrophobic film.
[0022] Furthermore, in the preparation method of the above-mentioned photothermal hydrophobic film, the light-absorbing filler can be at least one of metals or metal oxides such as copper, silver, and gold, semiconductors such as titanium trioxide, molybdenum disulfide, and copper sulfide, and carbon materials such as graphite, activated carbon, carbon black, carbon nanotubes, graphene, graphene oxide, and two-dimensional transition metal carbides; but it is not limited to this.
[0023] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the base material includes: fabric, non-woven fabric or thin sponge, etc.
[0024] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the low surface energy hydrophobic polymer material is selected from: polydimethylsiloxane, methyltrichlorosilane, dodecafluoroheptylpropyltrimethoxysilane, octyltrimethoxysilane, fluorosilane or phenyltrichlorosilane, etc.
[0025] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the curing agent is selected from: diphenylbutyl carbamate, dibutyl phthalate or diethylenetriamine or triethylenetetramine, etc.
[0026] Furthermore, the preparation method of the photothermal hydrophobic film is: first ultrasonically disperse the light-absorbing filler in the solvent 1 to form a photothermal filler solution (a surfactant may also be added for better dispersion), then immerse the base material in the solution, and use ultrasonic deposition to coat the light-absorbing filler on the base; dry it, then immerse it in a solvent 2 of a low surface energy hydrophobic polymer material and a curing agent, and finally take it out and heat it for curing.
[0027] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic membrane, the concentration of the photothermal filler solution is 1 to 20 g / L.
[0028] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the time for the ultrasonic deposition to coat the photothermal filler on the substrate is 2 to 3 hours.
[0029] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the mass ratio of the low surface energy hydrophobic polymer material to the curing agent is 1:1 to 10:1, and the mass ratio of the low surface energy hydrophobic polymer material to the solvent 2 is 1:100 to 3:100.
[0030] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the solvent 1 is selected from: water, ethanol, methanol, N,N-dimethylformamide or dimethyl sulfoxide.
[0031] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the solvent 2 is selected from: toluene, n-hexane, n-heptane, benzene or diethyl ether.
[0032] Furthermore, in the above-mentioned method for preparing the photothermal hydrophobic film, the temperature of the heating curing is 20 to 80° C., and the curing time is 5 to 10 hours.
[0033] In the present invention, the size and thickness of the photothermal hydrophobic film can be adjusted during actual use, and can be folded into different shapes, such as flower shape, zigzag shape, but not limited thereto.
[0034] Further, the heat insulating layer may be polyvinyl chloride foam, polystyrene foam, ethylene-vinyl acetate copolymer material, polyurethane foam, etc., but is not limited thereto.
[0035] The second technical problem to be solved by the present invention is to provide a preparation method for the above-mentioned integrated multifunctional solar evaporator, which is: firstly placing the hydrophilic aerogel in the photothermal hydrophobic film and the thermal insulation layer in sequence, so that the hydrophilic aerogel continuously penetrates the photothermal hydrophobic film and the thermal insulation layer, and then connecting two electrodes at the upper and lower ends of the hydrophilic aerogel.
[0036] The third technical problem to be solved by the present invention is to provide a method for using the above-mentioned integrated multifunctional solar evaporator, wherein the integrated multifunctional solar evaporator is immersed in seawater or fresh water, and when in use, the hydrophilic aerogel and the photothermal hydrophobic film are both located above the water surface.
[0037] Beneficial effects of the present invention:
[0038] 1) The present invention uses hydrophilic polymer as raw material, adopts ice template and freeze drying method, and prepares aerogel containing oxygen-containing functional groups and having a stable vertically oriented three-dimensional porous structure. This oriented structure is not only conducive to the transmission of evaporator water and the escape of evaporation, but also helps to improve its mechanical properties in order to achieve long-term use.
[0039] 2) The prepared aerogel evaporator has the advantages of a wide absorption range in the solar spectrum and high photothermal conversion efficiency.
[0040] 3) The present invention introduces a hydrophobic photothermal film around the vertically oriented aerogel. Due to the difference in wettability between the hydrophobic film and the hydrophilic aerogel, a temperature gradient is formed under light. The heat on the high-temperature hydrophobic photothermal film is continuously transferred to the low-temperature aerogel through its thermal conductive network, thereby achieving a better balance between rapid water supply and rapid heat supply, and accelerating the evaporation of the evaporator.
[0041] 4) The solar evaporator described in the present invention has high photothermal conversion efficiency, high evaporation rate, good salt resistance, and can generate electricity to the greatest extent while quickly producing clean water. The preparation method described is simple, the conditions are mild, and the price is low. It has broad application prospects in the fields of seawater desalination, sewage treatment, solution purification, wet gas power generation, photothermal power generation, or in solar cookers, heating furnaces, dryers and other devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is the SEM result of the aerogel obtained in Example 1 of the present invention.
[0043] Figure 2 This is a diagram showing the water transport state of the aerogel obtained in Example 1 of the present invention changing with time.
[0044] Figure 3 The water contact angle test results of the CCP composite membrane in the embodiment.
[0045] Figure 4 The CCP membrane obtained in the implementation is 1kW / m 2 The surface temperature changes with time under xenon light.
[0046] Figure 5 The results of the stability test of the evaporator obtained in Example 1 of the present invention by conducting a continuous evaporation experiment in seawater for 10 hours are shown.
[0047] Figure 6 This is the SEM result of the aerogel obtained in Comparative Example 1 of the present invention.
[0048] Figure 7 This is a diagram showing the water transport state of the aerogel obtained in Comparative Example 1 of the present invention as a function of time.
[0049] Figure 8 The results of the stability test of the evaporator obtained in comparative example 3 of the present invention in seawater after continuous evaporation for 10 hours are shown.
[0050] Fig. 9 Schematic diagram of the process for preparing vertically oriented aerogel in an embodiment of the present invention.
[0051] Fig.10 It is a process principle diagram for preparing the photothermal hydrophobic film in an embodiment of the present invention.
[0052] Fig.11 It is a schematic diagram of the structure of solar hot water evaporation and moisture power generation in an embodiment of the present invention.
[0053] Fig.12 This is a physical diagram of the integrated system of solar hot water evaporation and wet gas power generation in an embodiment of the present invention.
[0054] Fig.13 It is a schematic diagram of the randomly arranged structure solar evaporator obtained in Comparative Example 1 of the present invention.
[0055] Fig.14 It is a schematic diagram of the vertically oriented structure solar evaporator obtained in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0056] The present invention provides a new type of solar evaporator with gradient heating effect based on multi-level carbon nanotubes and utilizing the difference in hydrophilicity. The evaporator is composed of a hydrophilic PDA@CNT / PVA aerogel with a vertically oriented structure as a water evaporation layer, and a surrounding hydrophobic CCP film as a heating layer. The VA-PDA@CNT / PVA aerogel utilizes its ultra-high porosity, high specific surface area, and short water transport path to drive rapid water transportation during the solar evaporation process, and utilizes its strong light absorption capacity (the entire sunlight spectrum absorbs up to 98.2%) to perform photothermal conversion for evaporation and heat absorption. At the same time, the hydrophilic aerogel and the hydrophobic CCP film form a stable temperature gradient of nearly 70°C, so that the heat on the high-temperature CCP film is continuously and rapidly transferred to the low-temperature aerogel through its heat conduction network, thereby achieving a perfect balance between rapid water supply and rapid heat supply. In 5.0wt% NaCl (higher than the world's average seawater salinity of 3.5wt%) salt water, the water evaporation rate is as high as 6.96kg m under one sunlight. -2 h -1,At the same time, the high-flux directional flow of salt water induced by evaporation passes through the ion channels in the aerogel channels, generating a stable voltage of 130mV and a short-circuit current of 120uA. By connecting the evaporators in series, the stored electricity is used to light up small electronic devices such as light-emitting diodes (LEDs). And the VA-PDA@CNT / PVA with CCP film evaporator has shown good stability in 5.0wt% NaCl for 7 consecutive days. More importantly, the evaporator was tested in real Bohai Sea water under natural light for 8h, and the fresh water it produced can meet the recommended daily drinking water intake of 2.6 households, and the power generation voltage has been above 60mV. The evaporator shows good adsorption capacity for dye molecules. This simple and new solar thermal interface evaporation structure is universal and suitable for the assembly of gradient thermal structures of most solar thermal materials, providing a new method for maximizing the use of solar energy for fresh water and power generation.
[0057] The present invention continuously penetrates the prepared vertically arranged aerogel through the photothermal hydrophobic film and the thermal insulation layer, wraps two electrodes on the sides of the upper and lower ends of the aerogel, and immerses it in seawater. The vertically arranged hydrophilic aerogel drives the rapid transportation of water, and uses its strong light absorption ability to perform photothermal conversion for evaporation and heat absorption. At the same time, the temperature gradient formed by the hydrophobic photothermal film and the hydrophilic aerogel under sunlight causes the heat on the high-temperature hydrophobic photothermal film to be continuously and rapidly transferred to the low-temperature aerogel, thereby achieving a better balance between rapid water supply and rapid heat supply. At the same time, the brine with high-flux directional flow induced by evaporation generates electricity through the ion channels in the aerogel channels, so that the evaporator can achieve high evaporation rate and good salt tolerance while maximizing power generation.
[0058] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.
[0059] The present invention will be described in detail below in conjunction with specific examples, but it is worth noting that those skilled in the art will understand that the following examples are only applicable to illustrating the present invention and should not be considered as limiting the scope of the present invention. In the case of no specific conditions, the normal conditions or conditions recommended by the manufacturer in the examples will be adopted, and the instruments or reagents used without indicating the manufacturer can be purchased commercially.
[0060] Example 1 Preparation of VA-PDA@CNT / PVA with CCPfilm Evaporator
[0061] The specific steps for preparing vertically oriented polyvinyl alcohol (PVA) aerogel are as follows: first, PVA particles are added to deionized water and dissolved at 90°C to prepare a 30 mg / ml PVA solution. The PDA@CNT hybrid is ultrasonically dispersed in an aqueous solution to prepare a 30 mg / ml PDA@CNT dispersion. Secondly, 10 g of PVA solution is taken and added dropwise to 10 g of PDA@CNT dispersion. Stir for 3 hours on a stirring table at 1000 rpm and then ultrasonicate for 10 minutes to prepare a precursor solution; then pour it into a mold with polytetrafluoroethylene on all sides and a copper bottom, and contact the bottom of the mold with a -110°C liquid nitrogen bath until the precursor solution is completely frozen. The resulting gel is freeze-dried at -50°C and 1 Pa for 48 hours to obtain an aerogel. The resulting aerogel is recorded as VA-PDA@CNT / PVA; the schematic diagram of the aerogel preparation process is shown in the figure Fig. 9 As shown. The above polydopamine (PDA) modified carbon nanotube (CNT) hybrid (PDA@CNT) is prepared by the following specific steps: First, weigh 1g of CNT and add it to 500ml of deionized water and ultrasonicate to evenly disperse the CNT. Then add 0.61g of tris(hydroxymethyl)aminomethane (Tris) to the above solution and stir it magnetically until dissolved, and adjust the pH of the solution to 8.5, then add 1g of dopamine (DA) to react for 2h. Finally, the PDA / CNT reaction solution is filtered, washed and dried to obtain the PDA@CNT hybrid.
[0062] The prepared aerogels were characterized by scanning electron microscopy. Figure 1 As shown in Figure 2, it can be seen that VA-PDA@CNT / PVA aerogel has a highly ordered oriented structure with vertical channels connecting the evaporation surface and the bulk water below, which makes the water transport path shorter and the time required for water transport shorter ( Figure 2 ).
[0063] The preparation steps of cotton cloth / carbon nanotube / polydimethylsiloxane photothermal hydrophobic film are as follows: First, add 5g CNT and 0.5g sodium dodecylbenzene sulfonate to 500ml deionized water, and perform strong ultrasonic treatment for 5h to form a stable 10g / L CNT suspension. Then immerse the pure cotton cloth in the CNT suspension (CNT / H2O dispersion), and use ultrasonic deposition method to coat the CNT on the pure cotton cloth. Next, dry the cotton cloth at 90°C to obtain a Cotton / CNT composite film. Then immerse the Cotton / CNT composite film in a 1wt% PDMS / butyl diphenylcarbamate / n-hexane solution (PDMS / butyl diphenylcarbamate (10 / 1, wt / wt), and finally take it out and dry it at 80°C for 5h to obtain a hydrophobic photothermal Cotton / CNT / PDMS (CCP) composite film; the schematic diagram of the preparation process of the hydrophobic photothermal composite film is shown in Fig.10 shown.
[0064] The prepared CCP composite film was tested using a contact angle tester. Figure 3 As shown in the figure, it can be seen that the water contact angle of the CCP membrane is 141°, showing obvious hydrophobicity. 2 The surface temperature curve under the xenon light changes with time, such as Figure 4 As shown, it can be seen that its surface temperature rises rapidly, reaching 90°C in 6s and then tends to stabilize. The surface temperature of the sample is as high as 107.0°C.
[0065] Preparation of vertically oriented evaporator with CCP film (VA-PDA@CNT / PVAwith CCP film): A circular hole with a diameter of 20 mm was carved in the center of the insulating foam polystyrene and the photothermal hydrophobic film CCP, and the vertically oriented aerogel was inserted into the CCP film (the CCP film was tightly wrapped around the aerogel) and the polystyrene foam in turn, so that the aerogel passed through the CCP film and the polystyrene foam in turn, and two electrodes were wrapped around the sides of the upper and lower ends of the aerogel to prepare a solar evaporator. The obtained solar evaporator was placed in seawater to further study its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation, as shown in Tables 1 and 2. The stability of the evaporator was further tested by conducting a continuous evaporation experiment in seawater for 10 hours, as shown in Tables 1 and 2. Figure 5 The schematic diagram of the solar evaporator for solar hot water evaporation and moisture power generation is shown in Fig.11 As shown in the figure, the actual picture of the solar evaporator integrating light-heat water evaporation and moisture power generation is as follows Fig.12 shown.
[0066] Example 2
[0067] The specific steps for preparing vertically oriented polyethylene glycol / polyacrylamide aerogel are as follows: polyethylene glycol (PEG) and polyacrylamide (PAM) are dissolved to prepare 20 mg / ml solutions respectively, and the two solutions are mixed at a mass ratio of 1:3 for 5 hours to form a uniform polymer solution. Molybdenum disulfide (MoS2) light-absorbing filler is ultrasonically uniformly dispersed in an aqueous solution to prepare a MoS2 solution with a concentration of 10 mg / ml. 6 g of polyethylene glycol / polyacrylamide polymer solution is added dropwise with 4 g of MoS2 solution, and the precursor solution is prepared by stirring and mixing; the precursor solution is then poured into a mold with polytetrafluoroethylene on all sides and a copper bottom, and the bottom of the mold is exposed to a liquid nitrogen bath at -196°C until the precursor solution is completely frozen. The obtained gel is freeze-dried at -50°C and 1Pa for 48 hours, and the obtained aerogel is recorded as VA-MoS2 / PEG / PAM.
[0068] The preparation of the photothermal hydrophobic membrane in this embodiment is exactly the same as that in Example 1, but the photothermal hydrophobic membrane is folded into a petal shape with a bottom hole diameter of 20 mm, which is recorded as a flower-shaped CCP membrane.
[0069] The vertically oriented evaporator (VA-MoS2 / PEG / PAM with CCP film) with flower-shaped CCP film was prepared as follows: a circular hole with a diameter of 20 mm was carved in the center of the insulating foam polystyrene, and the vertically oriented aerogel was passed through the CCP film and the polystyrene foam in sequence, and two electrodes were wrapped around the sides of the upper and lower ends of the aerogel. The obtained solar evaporator was placed in seawater to further study its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation, as shown in Table 1.
[0070] Example 3
[0071] The specific steps for preparing vertically oriented polyacrylic acid aerogel are as follows: ultrasonically disperse two-dimensional transition metal carbide (Mxene) and graphene oxide (GO) in water to prepare 30 mg / ml solutions. Dissolve polyacrylic acid (PAA) to prepare a polymer solution with a concentration of 40 mg / ml. Take 4g of Mxene dispersion solution, add 6g of GO dispersion solution and 10g of PAA solution to it and stir and mix evenly. Then pour it into a mold with polytetrafluoroethylene around and copper at the bottom, contact the bottom of the mold with a liquid nitrogen bath at -196°C until the precursor solution is completely frozen, and freeze-dry the obtained gel at -50°C and 1Pa for 60h. The obtained aerogel is recorded as VA-Mxene / GO / PAA aerogel.
[0072] The preparation steps of polyurethane foam / titanium trioxide / polydimethylsiloxane photothermal hydrophobic membrane are as follows: first, 2g of titanium trioxide (Ti2O3) is ultrasonically dispersed in a solution of 100ml deionized water, and loaded on polyurethane (PU) foam by ultrasonic deposition method to prepare photothermal PU / Ti2O3 membrane. Then, the PU / Ti2O3 membrane is immersed in 3wt% PDMS n-hexane solution (PDMS / diphenylbutyl carbamate (10 / 3, wt / wt), and finally taken out and cured at 60℃ for 8h to obtain a hydrophobic photothermal PU / Ti2O3 / PDMS (PTP) composite membrane.
[0073] The vertically oriented evaporator with PTP film (VA--Mxene / GO / PAAwith PTP) was prepared as follows: a circular hole with a diameter of 20 mm was carved in the center of the insulating foam polystyrene and the photothermal hydrophobic film PTP, and the vertically oriented aerogel was passed through the PTP film and the polystyrene foam in turn, and two electrodes were wrapped around the sides of the upper and lower ends of the aerogel. The obtained solar evaporator was placed in seawater to further study its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation.
[0074] Example 4
[0075] Prepare polyethyleneimine (PEI) and sodium polystyrene sulfonate (PSA) solutions with a concentration of 50 mg / ml respectively, stir the two solutions at a mass fraction of 3:7 for 5 hours to form a uniform PEI / PSA polymer solution. Ultrasonic disperse graphene oxide (GO) and titanium dioxide (TiO2) in aqueous solution to prepare a 50 mg / ml dispersion. Take 8g of GO dispersion, add 2g of TiO2 dispersion to it, and then add 10g of PEI / PSA polymer solution to it and stir and mix evenly. Then pour it into a mold with polytetrafluoroethylene around and copper at the bottom, contact the bottom of the mold with a liquid nitrogen bath at -196°C until the precursor solution is completely frozen, freeze-dry the obtained gel at -50°C and 1Pa for 60 hours, and the obtained aerogel is recorded as VA-GO / TiO2 / PEI / PSA.
[0076] The preparation of the photothermal hydrophobic membrane in this embodiment is exactly the same as that in Example 3, which is a PTP composite membrane.
[0077] The vertically oriented evaporator with PTP film (VA-GO / TiO2 / PEI / PSAwith PTP) was prepared as follows: a circular hole with a diameter of 20 mm was engraved in the center of the insulating foam ethylene-vinyl acetate and the photothermal hydrophobic film PTP, and the vertically oriented aerogel was passed through the PTP film and the ethylene-vinyl acetate foam in sequence, and two electrodes were wrapped around the sides of the upper and lower ends of the aerogel. The obtained solar evaporator was placed in seawater to further study its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation, as shown in Table 1.
[0078] Example 5
[0079] The preparation of the vertically oriented aerogel in this embodiment is exactly the same as that in Example 4.
[0080] The preparation steps of nylon 6 / silver / trimethylfluorosilane photothermal hydrophobic membrane are as follows: first, 2g / L silver paste (Ag) solution is ultrasonically dispersed, and it is loaded on nylon 6 (PA6) fabric by ultrasonic deposition method to prepare PA6 / Ag photothermal membrane. Then the PA6 / Ag photothermal membrane is immersed in 5wt% trimethylfluorosilane toluene solution (FTS / diethylenetriamine (10 / 6, wt / wt), and finally it is taken out and cured at 70℃ for 8h to obtain a hydrophobic photothermal PA6 / Ag / FTS (PAF) membrane.
[0081] The preparation of the vertically oriented evaporator with PAF film (VA-GO / TiO2 / PEI / PSAwith PAF) is as follows: a circular hole with a diameter of 20 mm is engraved in the center of the insulating foam ethylene-vinyl acetate and the photothermal hydrophobic film PAF, and the vertically oriented aerogel is passed through the PAF film and the ethylene-vinyl acetate foam in sequence, and two electrodes are wrapped around the sides of the upper and lower ends of the aerogel. The obtained solar evaporator is placed in seawater to further study its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation, as shown in Table 1.
[0082] After testing, the photothermal temperature, water evaporation rate, power generation current, and power generation voltage test comparison of the solar evaporators obtained in Examples 1 to 5 are shown in Table 1 below.
[0083] Table 1 Test results of photothermal temperature, water evaporation rate, power generation current and power generation voltage of solar evaporator obtained from Examples 1 to 5
[0084]
[0085] Comparative Example 1
[0086] The difference between this comparative example and Example 1 is that the same precursor solution is poured into a hollow copper column and placed in a refrigerator at -20°C to prepare a gel, and then freeze-dried for 48 hours at -50°C and 1 Pa. At this time, the temperature has no directionality, and a disordered aerogel can be formed, which is recorded as R-PDA@CNT / PVA aerogel.
[0087] The prepared aerogels were characterized by SEM. Figure 6 As shown in Figure 2, it can be seen that the R-PVA / PDA@CNT aerogel has a highly curved and wrinkled pore structure, which makes the water transport path from the bottom to the evaporation surface longer and takes longer time to transport ( Figure 7 ).
[0088] Another difference between this comparative example and Example 1 is that this comparative example does not have the preparation of photothermal hydrophobic film. Preparation of Randomly Arranged Evaporator Aerogel (R-PDA@CNT / PVA) According to the preparation method of the evaporator in Example 1, the disordered structure aerogel is penetrated through the polystyrene foam, and two electrodes are wrapped around the upper and lower sides of the aerogel. The obtained solar evaporator is placed in seawater to further study its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation, as shown in Table 2. The schematic diagram of the randomly arranged solar evaporator in this comparative example is shown in Fig.13 shown.
[0089] Comparative Example 2
[0090] The difference between this comparative example and Example 1 is that: this comparative example does not have the preparation of photothermal hydrophobic film. Preparation of vertically oriented aerogel evaporator (VA-PDA@CNT / PVA) According to the preparation method of the evaporator in Example 1, the vertically arranged aerogel is penetrated through the polystyrene foam, and two electrodes are wrapped around the sides of the upper and lower ends of the aerogel. The obtained solar evaporator is placed in seawater, and its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation are further studied, as shown in Table 2. The schematic diagram of the vertically oriented structure solar evaporator in this comparative example is shown in Fig.14 shown.
[0091] Comparative Example 3
[0092] The difference between this comparative example and Example 1 is that the same precursor solution is poured into a hollow copper column and placed in a refrigerator at -20°C to prepare a gel, and then freeze-dried for 48 hours at -50°C and 1 Pa. At this time, the temperature has no directionality, and a disordered aerogel can be formed, which is recorded as R-PDA@CNT / PVA aerogel.
[0093] Preparation of random arrangement evaporator with CCP film (R-PDA@CNT / PVAwith CCP film) According to the preparation method of the evaporator in Example 1, the randomly arranged aerogels were sequentially penetrated through the CCP film and polystyrene foam, and two electrodes were wrapped around the sides of the upper and lower ends of the aerogels. The obtained solar evaporator was placed in seawater to further study its water evaporation rate, photothermal conversion temperature and power generation performance under simulated 1 sun irradiation, as shown in Table 2. The evaporator was further tested for its stability by a continuous evaporation experiment in seawater for 10 hours. Figure 8 shown.
[0094] After testing, the photothermal temperature, water evaporation rate, power generation current, and power generation voltage of the solar evaporator obtained in Example 1 and Comparative Examples 1 to 3 are compared as shown in Table 2 below:
[0095] Table 2 Test results of photothermal temperature, water evaporation rate, power generation current and power generation voltage of the solar evaporator obtained in Example 1 and Comparative Examples 1 to 3
[0096]
[0097] The evaporation performance of the solar evaporator of the present invention is tested as follows: at an experimental temperature of 20°C, a humidity of 40%, and a convection speed of 0 ms -1 A series of comparative experiments were conducted under convection conditions. For the evaporation of aerogel evaporator without CCP film, each sample was irradiated under one sun for 1h or 10h (salt resistance), and the mass change of water during evaporation was recorded synchronously with a high-precision (0.1mg) analytical balance. In order to avoid the influence of direct evaporation of bulk water in the bottom layer on the test results, a circular hole with a diameter of 20mm was engraved in the center of the insulating foam, and the aerogel square was placed in it. Then, they were placed in a petri dish filled with water for water evaporation experiments. The heights of the aerogel immersed in water and exposed to the outside were 15mm and 25mm, respectively. In addition, during the evaporation process, the temperatures of five different points on the surface and side of the evaporator were recorded simultaneously using an infrared thermal imager (FLIR-T600) and the average was taken to obtain the temperature of the surface and side of the evaporator. For the evaporation of aerogel evaporator with CCP film, the CCP film was placed flat on the EPS foam and tested under the same conditions using the same method. The open circuit voltage and short circuit current of the solar evaporator were measured by a digital multimeter (Owon B35T+).
Claims
1. An integrated multifunctional solar evaporator, It is characterized in that The evaporator comprises a water evaporation layer, a heating layer and a heat-insulating layer, wherein the water evaporation layer is a hydrophilic aerogel having a vertically oriented structure, the water evaporation layer continuously and sequentially penetrates the heating layer and the heat-insulating layer, and the heating layer is a photothermal hydrophobic film; wherein the hydrophilic aerogel refers to a hydrophilic aerogel having a vertically oriented structure which is prepared by using a hydrophilic polymer as a matrix and a light-absorbing material as a filler; and the content of the light-absorbing material in the hydrophilic aerogel is 10-70wt%.
2. An integrated multifunctional solar evaporator according to claim 1, It is characterized in that The hydrophilic aerogel is a hydrophilic aerogel with a vertically oriented three-dimensional porous structure, which is prepared by using a hydrophilic polymer and a light-absorbing material as raw materials and adopting an ice template and a freeze-drying method.
3. An integrated multifunctional solar evaporator according to claim 1 or 2, It is characterized in that The heat insulating layer is made of polyvinyl chloride foam, polystyrene foam, ethylene-vinyl acetate copolymer material or polyurethane foam.
4. An integrated multifunctional solar evaporator according to claim 1 or 2, It is characterized in that The hydrophilic polymer includes at least one of polyvinyl alcohol, polyethylene glycol, polyacrylic acid, sodium polyacrylate, sodium polystyrene sulfonate, polyacrylamide, polyvinylamide or polyethyleneimine.
5. An integrated multifunctional solar evaporator according to claim 1 or 2, It is characterized in that The light absorbing material is a metal and its oxide, a semiconductor material or a carbon material.
6. The integrated multifunctional solar evaporator according to claim 5, It is characterized in that The light absorbing material is selected from at least one of the following substances: copper, silver, gold or metal oxides thereof, titanium trioxide, molybdenum disulfide or copper sulfide, polydopamine, graphite, activated carbon, carbon black, carbon nanotubes, graphene, graphene oxide or two-dimensional transition metal carbide.
7. The integrated multifunctional solar evaporator according to claim 1, It is characterized in that The hydrophilic aerogel is prepared by the following method: firstly, a hydrophilic polymer solution and a light absorbing material are uniformly mixed to obtain a precursor solution; and then the precursor solution is subjected to an ice template and freeze-drying method to obtain a hydrophilic aerogel with a vertically oriented structure.
8. The integrated multifunctional solar evaporator according to claim 7, It is characterized in that The hydrophilic aerogel is prepared by the following method: firstly, a hydrophilic polymer is prepared into a hydrophilic polymer solution; then, a light absorbing material is ultrasonically dispersed in the hydrophilic polymer solution and mixed to obtain a precursor solution; The precursor solution is then poured into a mold with polytetrafluoroethylene on the sides and copper on the bottom. The mixed solution in the mold is frozen into shape using an ice template directional preparation process. It is then vacuum freeze-dried to produce a hydrophilic aerogel with a vertically oriented structure.
9. The integrated multifunctional solar evaporator according to claim 8, It is characterized in that The concentration of the hydrophilic polymer solution is 20-50 mg / ml.
10. An integrated multifunctional solar evaporator according to claim 8 or 9, It is characterized in that During the freezing molding process, the freezing temperature is -196 to -78°C, and the freezing time is 180 to 300 minutes.
11. An integrated multifunctional solar evaporator according to claim 8 or 9, It is characterized in that The vacuum freeze-drying time is 48~72h.
12. The integrated multifunctional solar evaporator according to claim 1, It is characterized in that The photothermal hydrophobic film is prepared by the following method: coating a light-absorbing filler on a base material, immersing the base material in a solution containing a low-surface-energy hydrophobic polymer material and a curing agent after drying, and finally curing the base material to obtain the photothermal hydrophobic film.
13. The integrated multifunctional solar evaporator according to claim 12, It is characterized in that The light-absorbing filler is a metal and its oxide, a semiconductor material or a carbon material.
14. The integrated multifunctional solar evaporator according to claim 13, It is characterized in that The light-absorbing filler is selected from: copper, silver, gold or metal oxides thereof, titanium trioxide, molybdenum disulfide or copper sulfide, polydopamine, graphite, activated carbon, carbon black, carbon nanotubes, graphene, graphene oxide or two-dimensional transition metal carbide.
15. The integrated multifunctional solar evaporator according to claim 12, It is characterized in that The base material includes: fabric, non-woven fabric or sponge.
16. The integrated multifunctional solar evaporator according to claim 12, It is characterized in that The low surface energy hydrophobic polymer material is selected from: polydimethylsiloxane, methyltrichlorosilane, dodecafluoroheptylpropyltrimethoxysilane, octyltrimethoxysilane, fluorosilane or phenyltrichlorosilane.
17. The integrated multifunctional solar evaporator according to claim 12, It is characterized in that The curing agent is selected from: diphenyl butyl carbamate, dibutyl phthalate or diethylenetriamine or triethylenetetramine.
18. An integrated multifunctional solar evaporator according to claim 12, It is characterized in that The preparation method of the photothermal hydrophobic film is as follows: firstly, ultrasonically disperse the light-absorbing filler in solvent 1 to form a photothermal filler solution, then immerse the substrate material in the solution, and use ultrasonic deposition to coat the light-absorbing filler on the substrate; dry it, then immerse it in solvent 2 including a low surface energy hydrophobic polymer material and a curing agent, and finally take it out and heat it for curing; wherein, the solvent 1 is selected from: water, ethanol, methanol, N,N-dimethylformamide or dimethyl sulfoxide; the solvent 2 is selected from: toluene, n-hexane, n-heptane, benzene or ether.
19. An integrated multifunctional solar evaporator according to claim 18, It is characterized in that The concentration of the photothermal filler solution is 1-20 g / L.
20. An integrated multifunctional solar evaporator according to claim 18, It is characterized in that The mass ratio of the low surface energy hydrophobic polymer material to the curing agent is 1:1-10:1, and the mass ratio of the low surface energy hydrophobic polymer material to the solvent 2 is 1:100-3:
100.
21. An integrated multifunctional solar evaporator according to claim 18, It is characterized in that The temperature of the heating curing is 20-80° C., and the curing time is 5-10 hours.
22. A method for preparing an integrated multifunctional solar evaporator according to any one of claims 1 to 21, It is characterized in that The preparation method is as follows: firstly, the hydrophilic aerogel is sequentially placed in the photothermal hydrophobic film and the thermal insulation layer, so that the hydrophilic aerogel continuously penetrates the photothermal hydrophobic film and the thermal insulation layer, and then two electrodes are connected at the upper and lower ends of the hydrophilic aerogel.
23. A method for using the integrated multifunctional solar evaporator according to any one of claims 1 to 21, It is characterized in that The integrated multifunctional solar evaporator is immersed in seawater or fresh water, and the hydrophilic aerogel and the photothermal hydrophobic film are both located above the water surface during use.