A method for recycling sulfuric acid in a chip factory to prepare high-purity copper sulfate in an environmentally friendly manner

By recycling and processing electronic-grade sulfuric acid, high-purity copper sulfate is prepared by dilution, ion exchange resin purification, electrocatalytic oxidation and electrolysis processes, the problems of waste of electronic-grade sulfuric acid resources and the demand of semiconductor industry are solved, and high-efficiency and environmentally friendly copper sulfate is achieved. preparation.

CN117210822BActive Publication Date: 2024-11-22CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311067443.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-23
Publication Date
2024-11-22
Estimated Expiration
2043-08-23

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently utilize electronic-grade sulfuric acid, resulting in waste of resources and high environmental protection costs, and the demand for high-purity copper sulfate in the semiconductor industry is difficult to meet.

Method used

By recycling the cleaned SPM waste liquid, dilution, ion exchange resin purification, electrocatalytic oxidation and electrolysis processes, a high-purity copper sulfate solution was prepared, and silver sulfate was generated using the anode metal copper plate in the electrolytic cell.

Benefits of technology

It realizes the preparation and efficient utilization of high-purity copper sulfate, reduces environmental protection costs, and meets the semiconductor industry's demand for high-purity copper sulfate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117210822B_ABST
    Figure CN117210822B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner. For the SPM waste liquid generated in the chip manufacturing process, the present invention first pre-treats it, then uses a chaotic circuit to electrocatalytically oxidize it, and then feeds it into an electrolytic cell to electrolyze and prepare copper sulfate using a high-purity copper sheet as an anode. The copper sulfate solution after electrolysis can be filtered through a microporous membrane, evaporated and concentrated, and cooled and crystallized to obtain high-purity copper sulfate that meets the electroplating grade requirements for chip packaging. The process of the present invention is simple, and the mixed waste liquid of sulfuric acid and hydrogen peroxide generated by the chip factory is comprehensively utilized. The electrolytic process is used to prepare electroplating-grade high-purity copper sulfate for semiconductor packaging, turning waste into treasure and forming a cascade and high-value utilization model of sulfur resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of environmental protection, in particular to the treatment of SPM (Surfuric / Peroxide Mi) waste liquid. Background Art

[0002] Electronic-grade sulfuric acid becomes a large amount of waste sulfuric acid after being used in the production processes of ultra-large-scale integrated circuits, liquid crystal displays, and LEDs. At present, the global consumption of electronic-grade sulfuric acid has reached 1.5 million tons. After being configured with SPM solution, its amount reaches more than 1.8 million tons. Due to its difficulty in processing and high environmental protection requirements, its processing cost is increasing, increasing the environmental protection burden and production and operation burden of enterprises. After being used, electronic-grade sulfuric acid mainly contains impurities such as metal ions, hydrogen peroxide, and organic matter. The waste liquid composition is complex, and the metal ion content of the product is as high as 100ppb.

[0003] At present, the chip factory waste sulfuric acid treatment method is harmless disposal. However, the sulfuric acid concentration of SPM waste liquid is high, and its quality is better than industrial sulfuric acid. Harmless disposal causes waste of resources. How to make high-quality use of these large amounts of waste liquid has become an important research direction.

[0004] On the other hand, high-purity copper sulfate is widely used. In certain processes in the semiconductor industry, CuSO 4 The formation of holes or gaps caused by insufficient purity will lead to serious reliability problems in three-dimensional packaged chips. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner, characterized in that the method comprises the following steps:

[0006] 1) Recover the SPM waste liquid after cleaning the wafer;

[0007] 2) diluting the SPM waste liquid, and subjecting the diluted SPM waste liquid to ion exchange resin purification treatment;

[0008] 3) sending the waste liquid treated in step 2) into an electrolysis tank and subjecting it to electrocatalytic oxidation;

[0009] 4) sending the waste liquid after electrolysis in step 3) to an electrolytic cell;

[0010] The anode of the electrolytic cell is a metal copper plate; during the electrolysis process in the electrolytic cell, the anode metal copper is dissolved to obtain copper sulfate.

[0011] Furthermore, in step 1), the SPM waste liquid is the SPM solution after cleaning the wafer in the chip manufacturing process; the SPM solution is prepared by electronic grade sulfuric acid and electronic grade hydrogen peroxide in a ratio of 4:1 or 5:1.

[0012] Furthermore, in step 1), the SPM waste liquid contains 60%-80% sulfuric acid, 0.02% hydrogen peroxide, and metal ions greater than 10 ppm, and the metal impurities include one or more metal ions such as iron, arsenic, titanium, zinc, and tungsten.

[0013] Furthermore, before the dilution in step 2), the waste liquid is first filtered through a microporous membrane to remove particles larger than 0.1 μm, and then diluted with ultrapure water; further, the microporous membrane filtration size is two combinations of 200 nm, 100 nm, 50 nm, and 30 nm, and after filtration, the 0.1 μm particle size is <500 pcs / ml.

[0014] Furthermore, in step 2), ultrapure water is added to dilute the SPM waste liquid.

[0015] Furthermore, in step 2), ultrapure water is added to dilute the SPM waste liquid to a sulfuric acid content of 55%-65%. Further, the diluted waste sulfuric acid solution is purified by ion exchange resin to remove metal ions in the waste sulfuric acid; preferably, the concentration of sulfuric acid in the waste liquid after release is 15%-30%, the metal ions in the ultrapure water used are less than 0.01ppb, and the hydrogen peroxide content in the diluted waste liquid is less than 0.005% to meet the requirements of the ion exchange resin;

[0016] Further, in step 2), the ion exchange resin is a "tough gel" strong base anion exchange resin with a polystyrene framework, further, the resin model is a combination of 1-3 of TulsimerA-853E, TulsimerA-32, Fine mesh, Dowex-1, lonacA-540, and Diaion-SA10A, further, the resin is activated with 5%, 10%, and 15% electronic grade sulfuric acid, respectively, and further, the quality of the waste liquid after removing metal ions reaches 1ppb.

[0017] Further, in step 3), before the electrocatalytic oxidation treatment, electronic grade hydrogen peroxide with a concentration of 32% is added, the volume ratio of the added electronic grade hydrogen peroxide to the waste liquid is 1:20-1:30, and the electronic grade hydrogen peroxide is G3 grade;

[0018] In step 3), the electrocatalytic oxidation oxidizes the polyvalent sulfur into sulfate and generates active oxygen, wherein the reaction includes:

[0019] 2SO 3 2- +O 2 →2SO 4 2- (1)

[0020] 2S 2 O 3 2-+3O 2 →2S 2 O 6 2- (2)

[0021] S 2 O 8 2- →O 2 +S 2 O 6 2- (3)

[0022] 2S 2 O 6 2- +O 2 +H 2 O→4SO 4 2- +4H + (4)

[0023] Further, in step 3), the electrocatalytic oxidation process parameters are: the current density of the electrode is 50A / m 2 -150A / m 2 The anode material is one of the following: a mixed metal oxide (MMO) coated titanium anode, a graphite electrode, an antimony-doped tin dioxide electrode, or a boron-doped diamond thin layer electrode, and the cathode material is graphite. After electrocatalytic oxidation, the content of low-valent sulfur such as sulfite and dithionate in the waste liquid is below 2ppm.

[0024] Furthermore, in step 3), a chaotic circuit is used to electrocatalytically oxidize the waste liquid.

[0025] Further, in step 3), the chaotic circuit adopts an amplitude-frequency modulation chaotic circuit system, and the current density on the electrode of the chaotic circuit is 50A / m 2 -150A / m 2 .

[0026] Further, in step 4), the two ends of the electrolytic cell are the anode chamber and the cathode chamber, and the middle is the intermediate chamber, wherein V (anode chamber): V (intermediate chamber): V (cathode chamber) = 1:4:1 to 1:6:1.

[0027] Furthermore, in step 4), the anode chamber and the middle chamber are separated by a sulfonic acid cation exchange membrane, and the cathode chamber and the middle chamber are separated by a composite membrane layer of a proton exchange membrane and a microporous polymer membrane group.

[0028] Further, in step 4), the electrolysis process parameters are: current density 300A / m 2 -400A / m 2 , the anode is a high-purity copper sheet and the cathode is a titanium plate;

[0029] Furthermore, during the electrolysis process, the intermediate chamber liquid is used to produce a copper sulfate solution, that is, during the electrolysis process, the intermediate chamber liquid is circulated by a pump, the copper sulfate solution is continuously produced, and dilute sulfuric acid is supplemented, so as to realize continuous preparation of the copper sulfate solution.

[0030] Furthermore, the copper sulfate solution after electrolysis is filtered through a microporous membrane and the concentration is adjusted to meet the requirements of the copper sulfate solution of chip packaging electroplating grade. Further, the copper sulfate solution prepared above is circulated and filtered through 50nm, 30nm, and 10nm microporous filtration membranes, and the filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals that meet the requirements of chip packaging electroplating grade.

[0031] It is worth mentioning that in the semiconductor industry, there is a great demand for high-purity copper sulfate solution.

[0032] However, it is difficult to effectively utilize a large amount of waste electronic-grade sulfuric acid in the prior art. The technical effect of the present invention is unquestionable, that is, waste electronic-grade sulfuric acid is used to prepare copper sulfate, which can be made into high-purity copper sulfate liquid. High-purity copper sulfate is returned to the chip factory for use, achieving high-value utilization. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a process flow chart for a chip factory to recycle sulfuric acid to prepare high-purity copper sulfate solution. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with the embodiments, but it should not be understood that the above subject matter of the present invention is limited to the following embodiments. Without departing from the above technical ideas of the present invention, various substitutions and changes are made according to the common technical knowledge and customary means in the art, which should all be included in the protection scope of the present invention.

[0035] In an embodiment of the present invention, a waste sulfuric acid solution having components of 60% sulfuric acid, 0.01% hydrogen peroxide, and metal ions>1ppm is filtered through a microporous membrane, and ultrapure water is added for dilution after filtration. The diluted waste sulfuric acid is purified by resin, and the resin is respectively activated by 5%, 10%, and 15% electronic grade sulfuric acid before use. An appropriate amount of 32% electronic grade hydrogen peroxide (G5 grade) is added to the diluted waste sulfuric acid solution, and then enters an electrocatalytic oxidation tank, wherein the electrocatalytic oxidation adopts a chaotic circuit, and the anode material is one of a mixed metal oxide (MMO) coated titanium anode, a graphite electrode, an antimony-doped tin dioxide point electrode, and a boron-doped diamond thin layer electrode, and the cathode material is graphite. The purified waste sulfuric acid enters the electrolytic cell, which adopts a three-chamber structure. The anode chamber and the middle chamber use sulfonic acid cation exchange membranes, and the cathode chamber and the middle chamber use proton exchange membranes and microporous polymer membranes. The initial copper sulfate solution is prepared by electrolysis with a high-purity copper sheet as the anode, and the cathode is a titanium plate. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and the copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to achieve continuous preparation of copper sulfate solution. The copper sulfate solution after electrolysis is circulated and filtered through a microporous filter membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals that meet the requirements of chip packaging electroplating level.

[0036] Example 1

[0037] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0038] (1) collecting the SPM waste liquid (waste sulfuric acid solution) after cleaning the wafer and filtering it through a 100nm+50+30nm three-level microporous membrane, and then adding ultrapure water to dilute it to 15% and the hydrogen peroxide content to 0.002%;

[0039] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0040] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0041] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(intermediate chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the intermediate chamber is circulated by a pump, and the copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain a copper sulfate solution;

[0042] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0043] Table 1:

[0044]

[0045] Example 2

[0046] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0047] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 20% and the hydrogen peroxide content is 0.002%;

[0048] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0049] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0050] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0051] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0052] Table 2

[0053]

[0054] Example 3

[0055] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0056] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 25% and the hydrogen peroxide content is 0.002%;

[0057] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0058] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0059] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0060] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0061] Table 3

[0062]

[0063]

[0064] Example 4

[0065] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0066] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0067] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Tulsimer A-32;

[0068] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0069] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0070] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0071] Table 4

[0072]

[0073] Example 5

[0074] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0075] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0076] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-32 and Dowex-1;

[0077] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0078] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0079] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0080] Table 5

[0081]

[0082] Example 6

[0083] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0084] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0085] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-32 and lonac A-540;

[0086] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0087] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0088] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0089] Table 6

[0090]

[0091] Example 7

[0092] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0093] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0094] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E, Tulsimer A-32, and Diaion-SA10A;

[0095] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0096] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0097] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0098] Table 7

[0099]

[0100]

[0101] Example 8

[0102] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0103] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0104] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0105] (3) Add 1 / 15 of the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0106] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0107] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0108] Table 8

[0109]

[0110] Example 9

[0111] This embodiment provides a method for a chip factory to recover sulfuric acid to prepare a high-purity copper sulfate solution, comprising the following steps:

[0112] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0113] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0114] (3) Add 1 / 20 of the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0115] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0116] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0117] Table 9

[0118]

[0119] Example 10

[0120] This embodiment provides a method for recycling sulfuric acid in a chip factory to prepare high-purity copper sulfate in an environmentally friendly manner, comprising the following steps:

[0121] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0122] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0123] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 100A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0124] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0125] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0126] Table 10

[0127]

[0128] Embodiment 11

[0129] This embodiment provides a method for recycling sulfuric acid in a chip factory to prepare high-purity copper sulfate in an environmentally friendly manner, comprising the following steps:

[0130] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0131] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0132] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 50A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0133] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 400 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0134] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0135] Table 11

[0136]

[0137] Example 12

[0138] This embodiment provides a method for recycling sulfuric acid in a chip factory to prepare high-purity copper sulfate in an environmentally friendly manner, comprising the following steps:

[0139] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0140] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0141] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0142] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 350 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0143] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0144] Table 12

[0145]

[0146]

[0147] Embodiment 13

[0148] This embodiment provides a method for recycling sulfuric acid in a chip factory to prepare high-purity copper sulfate in an environmentally friendly manner, comprising the following steps:

[0149] (1) The waste sulfuric acid solution is filtered through a 100nm+50+30nm three-stage microporous membrane, and after filtration, ultrapure water is added to dilute it to 15% and the hydrogen peroxide content is 0.002%;

[0150] (2) The diluted waste sulfuric acid is purified by two-stage resins of Tulsimer A-853E and Diaion-SA10A;

[0151] (3) Add 1 / 10 the volume of dilute sulfuric acid to the diluted waste sulfuric acid solution, and then enter the electrocatalytic oxidation tank at a current density of 150A / m 2 The chaotic circuit performs electrocatalytic oxidation;

[0152] (4) The purified waste sulfuric acid enters the electrolytic cell, where copper sulfate is electrolyzed using a high-purity copper sheet as the anode and a titanium plate as the cathode at a current density of 300 A / m 2 The volume ratio of the three chambers is V(anode chamber):V(middle chamber):V(cathode chamber)=1:6:1. During the electrolysis process, the solution in the middle chamber is circulated by a pump, and copper sulfate solution is continuously extracted and supplemented with dilute sulfuric acid to obtain copper sulfate solution;

[0153] (5) The copper sulfate solution is circulated and filtered through a 50nm+30nm+10nm three-stage microporous filtration membrane. The filtered copper sulfate solution is evaporated, concentrated, cooled and crystallized to obtain high-purity copper sulfate crystals.

[0154] Table 13

[0155]

[0156] Compared with Example 10, Example 11 and Example 12, the concentration of the copper sulfate solution obtained by electrolysis of Example 10 is greater than that of Example 11 and greater than that of Example 10, and the energy and time consumed for concentration are minimal.

Claims

1. A method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner, characterized in that: The following steps are involved: 1) Recovering the SPM waste liquid after cleaning the wafer; the SPM waste liquid is the SPM solution after cleaning the wafer in the chip manufacturing process; the SPM waste liquid contains 60% to 80% sulfuric acid, 0.02% hydrogen peroxide, and metal ions greater than 10ppm; 2) diluting the SPM waste liquid, and subjecting the diluted SPM waste liquid to ion exchange resin purification treatment, adding ultrapure water to dilute the SPM waste liquid to a sulfuric acid content of 15%, and the purification resin is TulsimerA-853E, Diaion-SA10A; 3) sending the waste liquid treated in step 2) into an electrolytic barrel and subjecting it to electrocatalytic oxidation. Before the electrocatalytic oxidation treatment, adding electronic grade hydrogen peroxide with a concentration of 32%, the volume ratio of the added electronic grade hydrogen peroxide to the waste liquid is 1:20-1:30, and the electronic grade hydrogen peroxide is of G3 grade. The electrocatalytic oxidation oxidizes the polyvalent sulfur into sulfate and generates active oxygen; 4) sending the waste liquid after electrolysis in step 3) to an electrolytic cell; the anode of the electrolytic cell is a metal copper plate; during the electrolysis process in the electrolytic cell, the anode metal copper is dissolved to obtain copper sulfate.

2. The method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner according to claim 1, characterized in that: In step 3), a chaotic circuit is used to electrocatalytically oxidize the waste liquid.

3. The method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner according to claim 2, characterized in that: In step 3), the chaotic circuit adopts an amplitude-frequency modulation chaotic circuit system.

4. The method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner according to claim 1, characterized in that: In step 4), the two ends of the electrolytic cell are the anode chamber and the cathode chamber, and the middle is the intermediate chamber.

5. The method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner according to claim 1, characterized in that: In step 4), the anode chamber and the middle chamber are separated by a sulfonic acid cation exchange membrane, and the cathode chamber and the middle chamber are separated by a composite membrane layer of a proton exchange membrane and a microporous polymer membrane group.

6. A method for preparing high-purity copper sulfate by recycling sulfuric acid in a chip factory in an environmentally friendly manner according to claim 5, characterized in that: In step 4), the intermediate chamber liquid during the electrolysis process adopts a copper sulfate solution.