A phosphorus-nitrogen-silicon composite resin and its preparation method and application

By using the copolymerization reaction of silicon polyamine, phosphorus compound and bridge agent in the phosphorus-containing nitrogen-silicon composite resin, a trapezoidal structure with high crosslinking is formed, and the problem of insufficient strength and wear resistance of the existing flame retardant is solved. High-performance flame retardant and mechanical performance improvements are achieved.

CN117229509BActive Publication Date: 2024-11-15GUANGZHOU SIC NEW MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202311043597.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-18
Publication Date
2024-11-15
Estimated Expiration
2043-08-18

AI Technical Summary

Technical Problem

Existing phosphorus-containing silicon silicon flame retardants have shortcomings in strength and wear resistance, and it is difficult to meet the needs of high-performance materials.

Method used

Copolymerization reaction is carried out using silicon-containing polyamines, phosphorus-containing compounds and bridge-building agents to form a phosphorus-containing nitrogen-containing silicon-containing composite resin with trapezoidal structure and high crosslinking. The dehydration reaction of primary amine groups and phosphorus-hydroxyl groups and secondary amine groups are carried out through the dehydration reaction of primary amine groups and phosphorus-hydroxy groups. The ladder effect of the ball improves the wear resistance and strength of the resin.

Benefits of technology

It achieves high crosslinking, excellent flame retardant effect, heat resistance and mechanical properties, enhances the wear resistance and mechanical properties of the substrate, and is suitable for a variety of polymer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004401640800000031
    Figure BDA0004401640800000031
  • Figure BDA0004401640800000101
    Figure BDA0004401640800000101
Patent Text Reader

Abstract

The present invention belongs to the technical field of flame retardants, and provides a phosphorus-nitrogen-silicon composite resin and a preparation method and application thereof. The raw materials for preparing the phosphorus-nitrogen-silicon composite resin include the following components: (A) a silicon-containing polyamine containing at least two primary amino groups; (B) a phosphorus-containing compound having at least two phosphorus hydroxyl groups that react with the primary amino groups; (C) a bridging agent having at least two secondary amine groups. The phosphorus-nitrogen-silicon composite resin provided by the present invention has three elements of phosphorus, nitrogen and silicon, which can synergistically achieve an excellent flame retardant effect. On the other hand, the phosphorus-nitrogen-silicon composite resin has a trapezoidal structure with a high degree of crosslinking, which can give the substrate better wear resistance, heat resistance and mechanical properties, etc., and can be used as a flame retardant, and can be widely used in polymer materials such as plastic flame retardant, textiles, synthetic fibers and fabric coating flame retardant, tape flame retardant, silicone rubber, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardancy, and specifically relates to a phosphorus-nitrogen-silicon composite resin and a preparation method and application thereof. Background Art

[0002] With the development of my country's economy, the output of polymer synthetic plastic products has increased day by day, and has been widely used in various industries. Most plastics such as PP, PA, PE, ABS, etc. are flammable, and flame retardants need to be added when used, which has also promoted the rapid development of the flame retardant industry. At present, my country's flame retardant industry is in a stage of rapid development and green transformation, and new green and environmentally friendly flame retardants have become the main direction of the flame retardant industry. Flame retardants are generally divided into halogen, inorganic, phosphorus, nitrogen, silicon and expansion types. Among them, phosphorus flame retardants have good thermal stability, low toxicity and little impact on the environment; nitrogen flame retardants have high flame retardant efficiency, good volatility, and produce less harmful gases, with the characteristics of non-toxic or low toxicity; and silicon flame retardants have the characteristics of high efficiency, halogen-free, low smoke, low toxicity, anti-drip, and little impact on the environment, and have become the widely concerned green and environmentally friendly flame retardants.

[0003] Patent CN115304636A discloses a phosphorus-nitrogen-containing organosilicon flame retardant, its preparation method and application. The phosphorus-nitrogen-containing organosilicon flame retardant is prepared using phenylsiloxane monomer, chlorinated trimellitic anhydride, amino compounds, organic phosphoric acid, etc. as raw materials, and has the synergistic effect of organic silicon benzene, and has the characteristics of good flame retardant effect, small addition amount and little impact on material properties.

[0004] Patent CN113817170A discloses a phosphorus-nitrogen-silicon intumescent flame retardant, a preparation method thereof, and an application thereof in rigid polyurethane foam. The phosphorus-nitrogen-silicon intumescent flame retardant is prepared using isocyanate alkyl alkoxy silane, tris(2-hydroxyethyl)isocyanurate, and phenylphosphonic dichloride as raw materials. The obtained flame retardant can exert a synergistic flame retardant effect among phosphorus, nitrogen, and silicon. An aromatic hybrid structure is introduced into the flame retardant, so that the rigid polyurethane foam material has excellent heat resistance, flame retardancy, and corrosion resistance, while having little effect on the mechanical properties of the material.

[0005] The flame retardant disclosed in the above prior art contains phosphorus, nitrogen and silicon, and has a good flame retardant effect. However, the above flame retardant still has problems such as low strength and poor wear resistance.

[0006] Therefore, developing a phosphorus-nitrogen-silicon composite resin with better strength and wear resistance is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0007] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a phosphorus-nitrogen-silicon composite resin and its preparation method and application. The phosphorus-nitrogen-silicon composite resin provided by the present invention has three elements of phosphorus, nitrogen and silicon, which can synergistically achieve an excellent flame retardant effect. On the other hand, the phosphorus-nitrogen-silicon composite resin has a trapezoidal structure with a high degree of crosslinking. Compared with a single-chain resin, the trapezoidal structure can make the phosphorus-nitrogen-silicon composite resin have better wear resistance and strength, and can give the substrate better wear resistance, heat resistance and mechanical properties.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a phosphorus-nitrogen-silicon composite resin, wherein the raw materials for preparing the phosphorus-nitrogen-silicon composite resin include the following components:

[0010] (A) a silicon-containing polyamine containing at least two primary amine groups;

[0011] (B) a phosphorus-containing compound having at least two phosphorus hydroxyl groups reactive with the primary amino group;

[0012] (C) A bridging agent having at least two secondary amine groups.

[0013] The present invention adopts a polyamine-containing silicon monomer and a phosphorus-containing compound to form a cross-linked body with a three-dimensional structure, and uses a bridging agent as a ladder support to connect the cross-linked bodies together to obtain a phosphorus-nitrogen-silicon composite resin with a ladder structure and a cross-linked structure. The phosphorus-nitrogen-silicon composite resin can give the substrate excellent flame retardant effect, strength, wear resistance, heat resistance and other properties.

[0014] Preferably, the molar ratio between the primary amino group and the secondary amino group in the preparation raw material is (0.2-5):1; for example, it can be 0.3:1; 0.4:1; 0.5:1; 0.8:1; 1:1; 1.2:1; 1.4:1; 1.6:1; 1.8:1; 2:1; 2.2:1; 2.4:1; 2.6:1; 2.8:1; 3:1; 3.2:1; 3.4:1; 3.6:1; 3.8:1; 4:1; 4.2:1; 4.4:1; 4.6:1; 4.8:1, etc.

[0015] Preferably, the molar ratio between the primary amino group and the phosphorus hydroxyl group in the preparation raw material is (0.5-4): (1.6-10.8); for example, (0.5-4) can be 0.6, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, etc.; (1.6-10.8) can be 2, 3, 4, 5, 6, 7, 8, 9, 10, etc.

[0016] Preferably, the hydroxyphosphorus nitrogen-containing silicone resin comprises a polymer of the following general structural formula (I):

[0017]

[0018] R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from substituted or unsubstituted straight or branched alkyl, substituted or unsubstituted aryl, hydroxyl, Any one of, wherein "*" represents a connection site;

[0019] Z1, Z2, Z3, and Z4 are each independently selected from hydrocarbons, wherein the hydrocarbons are substituted by one or more of -SiO-, -Si-, -O-, -NH-, intermixed, and at least intermixed with one or more -SiO-, -Si-;

[0020] The hydrocarbon is any one of a substituted or unsubstituted straight-chain or branched alkylene group, a substituted or unsubstituted arylene group, a substituted or unsubstituted cycloalkylene group, and -Ar1-L-Ar2-;

[0021] R9, R 10 , R 11 , R 12 Each is independently selected from any one of hydrogen, substituted or unsubstituted straight or branched alkyl, and substituted or unsubstituted aryl;

[0022] R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 , R 20 , R 21 , R 22 , R 23 , R 24 , R 25 , R 26 , R 27 , R 28 are independently selected from hydrocarbons, wherein the hydrocarbons are substituted by one or more of -SiO-, -Si-, -O-, -NH-, be mixed;

[0023] The hydrocarbon is any one of a substituted or unsubstituted straight-chain or branched alkylene group, a substituted or unsubstituted arylene group, a substituted or unsubstituted cycloalkylene group, and -Ar1-L-Ar2-;

[0024] R1, R2, R3, R4, R5, R6, R7, R8, R9, R 10 , R 11 , R 12 , R 13 , R 14, R 15 , R 16 , R 17 , R 18 , R 19 , R 20 , R 21 , R 22 , R 23 , R 24 , R 25 , R 26 , R 27 , R 28 The substituents in the substitution include any one of halogen, unsubstituted or halogenated C1-C6 straight or branched alkyl, hydroxyl, alkoxy, phenoxy, siloxane, tertiary amine, primary amine, and secondary amine;

[0025] n is an integer of 0-5, for example, 1, 2, 3, or 4.

[0026] Preferably, the silicon-containing polyamine of component (A) includes 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminobutyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(2-aminoethyl)-1,1-dimethyl-3,3-diethyl-disiloxane, 1,5-bis(2-aminoethyl)-1,1,3,3,5,5-hexamethyltrisiloxane, 1,3-bis-(2-aminoethylaminomethyl)tetramethyldisiloxane, 1-aminopropyl-5-aminoethyl-1,1,3,3,5,5-hexamethyltrisiloxane, 1,7-bis(2-aminoethyl)-1,1,3,3,5,5,7,7-octamethyltetrasiloxane, 1,3-bis( One or more of 1,3-bis(3-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-aminopropyl)-1,3-dimethyl-1,3-diphenyldisiloxane, 1,3-bis(3-aminobutyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-aminoethyl)-1,1,3,3-tetramethyldisiloxane, aminopropyl di-terminated polydimethylsiloxane (PDMS), 3-aminopropyl di-terminated hexamethyltrisiloxane (ATPDs), bis(4-aminophenoxy)dimethylsilane (APDS) and 1,3-bis(p-aminophenoxy)tetramethyldisiloxane (APTS).

[0027] Preferably, the phosphorus-containing compound of component (B) includes hexamethylenediaminetetramethylenephosphonic acid, aminotrimethylenephosphonic acid, hydroxyethylidenediphosphonic acid, and diethylenetriaminepentamethylenephosphonic acid.

[0028] More preferably, the phosphorus-containing compound of component (B) includes hydroxyethylidene diphosphonic acid.

[0029] Preferably, the component (C) bridging agent includes one or more of piperazine, 2-methylpiperazine, 2-ethylpiperazine, 2,3-dimethylpiperazine, and 2,3-diethylpiperazine.

[0030] Preferably, the prepared raw material further comprises a catalyst.

[0031] Preferably, the catalyst is 4-dimethylaminopyridine.

[0032] Preferably, the catalyst is added in an amount of 0.1-1 wt % of the total weight of the raw materials.

[0033] In a second aspect, the present invention provides a method for preparing the phosphorus-nitrogen-silicon composite resin as described in the first aspect, the preparation method comprising the following steps:

[0034] The composition is obtained by subjecting the component (A) silicon-containing polyamine, the component (B) phosphorus-containing compound and the component (C) bridging agent to a dehydration condensation reaction.

[0035] Preferably, the dehydration condensation reaction is carried out under vacuum and reduced pressure to remove water.

[0036] Preferably, the temperature of the dehydration condensation reaction is 80-120°C.

[0037] Preferably, the dehydration condensation reaction time is 2 to 12 hours.

[0038] Preferably, the dehydration condensation reaction is carried out in the presence of a catalyst.

[0039] Preferably, the catalyst comprises 4-dimethylaminopyridine.

[0040] In a third aspect, the present invention provides the use of the above-mentioned phosphorus-nitrogen-silicon composite resin or the phosphorus-nitrogen-silicon composite resin prepared according to the above-mentioned preparation method in the field of flame retardancy.

[0041] In a fourth aspect, the present invention provides a flame retardant, which includes the above-mentioned phosphorus-nitrogen-silicon composite resin or the phosphorus-nitrogen-silicon composite resin prepared according to the above-mentioned preparation method.

[0042] In a fifth aspect, the present invention provides a flame retardant material, the flame retardant material comprising a substrate and a flame retardant;

[0043] The flame retardant is the above-mentioned phosphorus-nitrogen-silicon composite resin or the phosphorus-nitrogen-silicon composite resin prepared according to the above-mentioned preparation method.

[0044] Preferably, the flame retardant is added in an amount of 3-15% of the total weight of the flame retardant material.

[0045] Preferably, the substrate is selected from any one of a plastic substrate, a textile, a synthetic fiber, an adhesive tape, and a silicone rubber.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] (1) The phosphorus-nitrogen-silicon composite resin provided by the present invention is prepared by copolymerizing a silicon-containing polyamine, a phosphorus-containing compound and a bridging agent, wherein the primary amine group in the silicon-containing polyamine can undergo a stepwise dehydration reaction with the phosphorus hydroxyl group in the phosphorus-containing compound to form a cross-linked bulk intermediate, and at the same time, the two secondary amine groups of the bridging agent can also undergo a dehydration reaction with the phosphorus hydroxyl group to form a ladder support, and finally a phosphorus-nitrogen-silicon composite resin with a highly cross-linked, ladder-shaped structure is obtained. Compared with a single-chain resin, the phosphorus-nitrogen-silicon composite resin with a ladder-shaped structure has better heat resistance, chemical stability and mechanical properties. The phosphorus-nitrogen-silicon composite resin has high contents of phosphorus, nitrogen and silicon, can synergistically achieve a higher flame retardant effect, and has a high degree of crosslinking, excellent strength, hardness and mechanical properties. It not only does not have a negative impact on the mechanical properties and hardness of the substrate, but also can improve the wear resistance and performance of the substrate, and can be widely used in polymer materials such as plastic flame retardancy, textiles, synthetic fibers and fabric coating flame retardancy, tape flame retardancy, silicone rubber, etc., to improve the flame retardancy and wear resistance of polymer materials.

[0048] (2) The phosphorus-nitrogen-silicon composite resin provided by the present invention has abundant organic silicon segments, which can make the resin flexible while having a high degree of crosslinking, and can give the resin better water resistance. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0050] Example 1

[0051] A phosphorus-nitrogen-silicon composite resin is prepared by raw materials comprising: 24.9 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 30.9 g of hydroxyethylidene diphosphonic acid, 8.6 g of piperazine and 0.6 g of 4-dimethylaminopyridine.

[0052] A phosphorus-nitrogen-silicon composite resin, the preparation method of which comprises the following steps:

[0053] In a reactor equipped with a stirrer and a thermometer, the raw materials are put into the reactor for mixing, the temperature is raised to 100°C, and after stirring for 0.5h, vacuum decompression and water removal are carried out. After keeping the temperature under vacuum decompression and water removal conditions for 4h, the material is discharged and cooled to obtain a phosphorus-nitrogen-silicon composite resin.

[0054] Example 2

[0055] A phosphorus-nitrogen-silicon composite resin is prepared from raw materials comprising: 24.9 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 27.2 g of ethylenediaminetetramethylenephosphonic acid, 4.7 g of 2-methylpiperazine and 0.275 g of 4-dimethylaminopyridine.

[0056] A phosphorus-nitrogen-silicon composite resin, the preparation method of which comprises the following steps:

[0057] In a reactor equipped with a stirrer and a thermometer, the raw materials are put into the reactor for mixing, the temperature is raised to 110°C, and after stirring for 0.5h, vacuum decompression and water removal are carried out. After keeping the temperature under vacuum decompression and water removal conditions for 8h, the material is discharged and cooled to obtain a phosphorus-nitrogen-silicon composite resin.

[0058] Example 3

[0059] A phosphorus-nitrogen-silicon composite resin is prepared from raw materials comprising: 29.9 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 23.3 g of aminotri(methylenephosphonic acid), 4.6 g of 2-ethylpiperazine and 0.46 g of 4-dimethylaminopyridine.

[0060] A phosphorus-nitrogen-silicon composite resin, the preparation method of which comprises the following steps:

[0061] In a reactor equipped with a stirrer and a thermometer, the raw materials are put into the reactor for mixing, the temperature is raised to 120°C, and after stirring for 0.5h, vacuum decompression and water removal are carried out. After keeping the temperature under vacuum decompression and water removal conditions for 6h, the material is discharged and cooled to obtain a phosphorus-nitrogen-silicon composite resin.

[0062] Example 4

[0063] A phosphorus-nitrogen-silicon composite resin is disclosed, which differs from Example 1 in that the amount of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is changed to 12.5 g, the molar ratio of the primary amino group to the secondary amino group in the preparation raw material is changed to 0.5:1, the molar ratio and amount of other components remain unchanged, and the phosphorus-nitrogen-silicon composite resin is prepared by the same preparation method as Example 1.

[0064] Example 5

[0065] A phosphorus-nitrogen-silicon composite resin is disclosed, which differs from Example 1 in that the amount of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is changed to 99.6 g, the molar ratio of the primary amino group to the secondary amino group in the preparation raw material is changed to 4:1, the molar ratios of other components remain unchanged, and the phosphorus-nitrogen-silicon composite resin is prepared by the same preparation method as Example 1.

[0066] Example 6

[0067] A phosphorus-nitrogen-silicon composite resin is disclosed, which differs from Example 1 in that the amount of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is changed to 4.98 g, the molar ratio between the primary amino group and the secondary amino group in the preparation raw material is changed to 0.2:1, the molar ratio or amount of other components remains unchanged, and the phosphorus-nitrogen-silicon composite resin is prepared by the same preparation method as Example 1.

[0068] Example 7

[0069] A phosphorus-nitrogen-silicon composite resin is disclosed, which differs from Example 1 in that the amount of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is changed to 124.5 g, the molar ratio between the primary amino group and the secondary amino group in the preparation raw material is changed to 5:1, the molar ratio or amount of other components remains unchanged, and the phosphorus-nitrogen-silicon composite resin is prepared by the same preparation method as Example 1.

[0070] Comparative Example 1

[0071] A phosphorus-nitrogen-silicon composite resin is disclosed. The difference between the embodiment 1 and the embodiment 1 is that piperazine is not added, the molar ratio or dosage of other components remains unchanged, and the phosphorus-nitrogen-silicon composite resin is prepared by the same preparation method as the embodiment 1.

[0072] Comparative Example 2

[0073] A phosphorus-nitrogen-silicon composite resin is disclosed, which differs from Example 1 in that 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is not added, the molar ratio or dosage of other components remains unchanged, and the phosphorus-nitrogen-silicon composite resin is prepared by the same preparation method as Example 1.

[0074] Performance Test:

[0075] The phosphorus-nitrogen-silicon composite resins obtained in the above-mentioned Examples 1-7 and Comparative Examples 1 and 2 were crushed with a jet mill to obtain phosphorus-nitrogen-silicon composite resin powders. 8 parts of the phosphorus-nitrogen-silicon composite resin powders, 92 parts of homopolypropylene, 0.2 parts of antioxidant (IrganOx1010), and 1.5 parts of compatibilizer (PP grafted with maleic anhydride, grafting rate ≥2.5%) were added to a high-speed mixer and stirred for 5 minutes. Then, the mixture was added to a twin-screw extruder and granulated at 180°C. The prepared masterbatch was prepared into test specimens according to the test standard. The mechanical properties, flame retardancy and wear resistance of the specimens were tested according to the following method. The homopolypropylene without adding the phosphoric acid-containing silicone resin powder was used as a blank group. The test results are shown in Table 1.

[0076] 1. Wear resistance: Test the mass wear of the test specimen according to GB / T 3960-2016 "Plastic Sliding Friction Wear Test Method". The lower the mass wear, the better the wear resistance of the test specimen.

[0077] 2. Flame retardancy:

[0078] (1) Oxygen index: The limiting oxygen index (LOI) is tested in accordance with GBT 2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2 Room temperature test".

[0079] (2) Vertical burning performance: tested according to UL94 standard, the sample size is 125mm×13.0mm×1.0mm (UL-94).

[0080] 3. Flexural modulus: The flexural modulus is tested in accordance with GB / T9341-2008 "Determination of flexural properties of plastics".

[0081] Table 1

[0082]

[0083] According to the data in Table 1, we can see that:

[0084] The phosphorus-nitrogen-silicon composite resins obtained in Examples 1 to 7 have excellent flame retardant properties and can impart good wear resistance and flexural modulus to plastics.

[0085] It can be seen from Examples 1 to 7 that when the molar ratio between the primary amino group and the secondary amino group is in the range of (0.5 to 4): 1, the comprehensive performance of the obtained product is better; and when the molar ratio between the primary amino group and the secondary amino group is in the range of (1 to 3): 1, the comprehensive performance of the obtained product is the best.

[0086] From the comparison between Example 1 and Comparative Example 1, it can be seen that when piperazine is not added for copolymerization, the obtained phosphorus-nitrogen-silicon composite resin does not have a trapezoidal structure, the flame retardancy of the obtained product is slightly reduced, and the wear resistance and flexural modulus are significantly reduced.

[0087] By comparing Example 1 and Comparative Example 2, it can be seen that when 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is not added for copolymerization, the obtained product does not contain silicone, which is not conducive to the formation of a carbon layer and the flame retardant properties are significantly reduced. On the other hand, due to the decrease in crosslinking density, the wear resistance and flexural modulus of the obtained product are significantly reduced.

[0088] The applicant declares that the present invention illustrates a phosphorus-nitrogen-silicon composite resin and its preparation method and application through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A phosphorus-nitrogen-silicon composite resin, characterized in that: The raw materials for preparing the phosphorus-nitrogen-silicon composite resin include the following components: a silicon-containing polyamine containing at least two primary amine groups; a phosphorus-containing compound having at least two phosphorus hydroxyl groups reactive with the primary amine group; a bridging agent having at least two secondary amine groups; The phosphorus-containing compound of component (B) includes one or more of hexamethylenediaminetetramethylenephosphonic acid, aminotrimethylenephosphonic acid, hydroxyethylidenediphosphonic acid, and diethylenetriaminepentamethylenephosphonic acid; The component (C) bridging agent includes one or more of piperazine, 2-methylpiperazine, 2-ethylpiperazine, 2,3-dimethylpiperazine, and 2,3-diethylpiperazine.

2. The phosphorus-nitrogen-silicon composite resin according to claim 1, characterized in that: The molar ratio between the primary amine group and the secondary amine group in the preparation raw material is (0.2-5):

1.

3. The phosphorus-nitrogen-silicon composite resin according to claim 1, characterized in that: The molar ratio between the primary amine group and the phosphorus hydroxyl group in the preparation raw material is (0.5-4): (1.6-10.8).

4. The phosphorus-nitrogen-silicon composite resin according to claim 1, characterized in that: The silicon-containing polyamine of component (A) includes 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminobutyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(2-aminoethyl)-1,1-dimethyl-3,3-diethyl-disiloxane, 1,5-bis(2-aminoethyl)-1,1,3,3,5,5-hexamethyltrisiloxane, 1,3-bis-(2-aminoethylaminomethyl)tetramethyldisiloxane, 1-aminopropyl-5-aminoethyl-1,1,3,3,5,5-hexamethyltrisiloxane, 1,7-bis(2-aminoethyl)-1,1,3,3,5,5,7,7-octamethyl One or more of tetrasiloxane, 1,3-bis(3-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(4-aminophenyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-aminopropyl)-1,3-dimethyl-1,3-diphenyldisiloxane, 1,3-bis(3-aminobutyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-aminoethyl)-1,1,3,3-tetramethyldisiloxane, aminopropyl di-terminated polydimethylsiloxane, 3-aminopropyl di-terminated hexamethyltrisiloxane, bis(4-aminophenoxy)dimethylsilane and 1,3-bis(p-aminophenoxy)tetramethyldisiloxane.

5. The phosphorus-nitrogen-silicon composite resin according to claim 1, characterized in that: The preparation raw materials also include a catalyst.

6. The phosphorus-nitrogen-silicon composite resin according to claim 5, characterized in that: The catalyst includes 4-dimethylaminopyridine.

7. The phosphorus-nitrogen-silicon composite resin according to claim 5, characterized in that: The amount of the catalyst added is 0.1-1 wt % of the total weight of the raw materials.

8. The method for preparing the phosphorus-nitrogen-silicon composite resin according to any one of claims 1 to 7, characterized in that: The steps include: The composition is obtained by subjecting the component (A) silicon-containing polyamine, the component (B) phosphorus-containing compound and the component (C) bridging agent to a dehydration condensation reaction.

9. The preparation method according to claim 8, characterized in that: The dehydration condensation reaction is carried out under the condition of vacuum decompression and water removal.

10. The preparation method according to claim 8, characterized in that: The temperature of the dehydration condensation reaction is 80-120°C.

11. The preparation method according to claim 8, characterized in that: The dehydration condensation reaction time is 2 to 12 hours.

12. The preparation method according to claim 8, characterized in that: The dehydration condensation reaction is carried out in the presence of a catalyst; the catalyst includes dimethylaminopyridine.

13. Use of the phosphorus-nitrogen-silicon composite resin according to any one of claims 1 to 7 or the phosphorus-nitrogen-silicon composite resin prepared by the preparation method according to any one of claims 8 to 12 in the field of flame retardancy.

14. A flame retardant, characterized in that: The invention comprises the phosphorus-nitrogen-silicon composite resin as described in any one of claims 1 to 7 or the phosphorus-nitrogen-silicon composite resin prepared by the preparation method as described in any one of claims 8 to 12.

15. A flame retardant material, characterized in that: Including substrate and flame retardant; The flame retardant is the phosphorus-nitrogen-silicon composite resin as described in any one of claims 1 to 7 or the phosphorus-nitrogen-silicon composite resin prepared by the preparation method as described in any one of claims 8 to 12.

16. The flame retardant material according to claim 15, characterized in that: The added amount of the flame retardant is 3-15% of the total weight of the flame retardant material.

Citation Information

Patent Citations

  • Intumescent flame retardant containing phosphorus, nitrogen and silicon, preparation method of intumescent flame retardant and application of intumescent flame retardant in rigid polyurethane foam

    CN113817170A

  • Organic silicon flame retardant containing phosphorus and nitrogen as well as preparation method and application of organic silicon flame retardant

    CN115304636A

  • Phosphorus-nitrogen-silicon intumescent flame retardant containing triazine ring and cage structure and synthesis method of intumescent flame retardant

    CN107417912A

  • Phosphorus-silicon-nitrogen ternary synergistic flame retardant and preparation method thereof

    CN110563954A

  • Nitrogen-phosphorus-silicon ternary halogen-free synergistic flame-retardant thermoplastic elastomer and preparation method thereof

    CN113956597A