Antibacterial and antifouling furniture board and its manufacturing process

Through the combination of graphene-modified iron-doped nano-titanium dioxide and dihydroxy-terminated polydimethylsiloxane, photocatalytic degradation and magnetic microstructure are formed. Combined with the antibacterial coating of antibacterial agents, it solves the problem of difficult and durable furniture boards to clean. The problem of poor wear and short-lasting antibacterial effect is achieved by highly effective anti-fouling, waterproof, oil-proof and antibacterial properties, extending the service life.

CN117264534BActive Publication Date: 2024-10-18上海拉迷家具有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311299486.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-09
Publication Date
2024-10-18
Estimated Expiration
2043-10-09

AI Technical Summary

Technical Problem

Existing furniture panels are difficult to clean during use, have poor wear resistance, have short-lasting antibacterial effects and are prone to develop drug resistance, and cannot effectively prevent microbial contamination.

Method used

Graphene-modified iron-doped nano-titanium dioxide is combined with dihydroxy-terminated polydimethylsiloxane to photocatalytically degrade pollutants and form a magnetic microstructure. It is combined with antibacterial agents to form an antibacterial coating to improve antifouling and antibacterial properties. .

Benefits of technology

It achieves efficient anti-fouling, waterproof, oil-proof and anti-bacterial properties of furniture panels, extends its service life and enhances its protection against bacteria.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of furniture board materials, and discloses an antibacterial and antifouling furniture board material and a manufacturing process thereof. The invention comprises the following steps: uniformly mixing dihydroxyl-terminated polydimethylsiloxane and graphene-modified iron-doped nano titanium dioxide to obtain an antifouling coating; applying the coating on the upper surface of the furniture board material after vacuum degassing, vertically placing two glass slides at both ends of the board material, and then covering the two glass slides with a polytetrafluoroethylene plate, and finally placing a magnet on the lower surface of the furniture board material, curing, and repeating the above steps on the lower surface to obtain an antifouling modified furniture board material; adding isocyanate and monohydroxyl-terminated polydimethylsiloxane into a solvent, adding a catalyst to react, and obtaining a prepolymer; adding di(trimethylolpropane) and an antibacterial agent into N,N-dimethylformamide, stirring uniformly, adding the prepolymer to react, and obtaining an antibacterial coating; pouring the antibacterial coating onto the surface of the antifouling modified furniture board material, curing, and obtaining an antibacterial and antifouling furniture board material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fireproofing and anticorrosion treatment of wood surfaces, in particular to an antibacterial and antifouling furniture board and a manufacturing process thereof. Background Art

[0002] It is inevitable that furniture panels will produce stains during daily use. They are difficult to clean and easily damage the material on the surface of the panels, which is time-consuming and laborious. The existing anti-fouling furniture panels have a rough surface due to the use of super hydrophobic and oleophobic materials, resulting in poor wear resistance. The coating is easily damaged during use and loses its anti-fouling performance, and has a short service life. In addition to the numerous stains in life, there is also microbial contamination. Existing antibacterial treatments often use physical blending to add antibacterial agents to polymers. This method not only has a short antibacterial effect, but also produces drug resistance, making it difficult to achieve efficient and long-lasting antibacterial properties.

[0003] Therefore, it is of great significance to invent an antibacterial and antifouling furniture plate. Summary of the invention

[0004] The purpose of the present invention is to provide an antibacterial and antifouling furniture board and a manufacturing process thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A process for producing an antibacterial and antifouling furniture plate comprises the following steps:

[0007] S1: Mix dihydroxy-terminated polydimethylsiloxane and graphene-modified iron-doped nano-titanium dioxide evenly to obtain an antifouling coating; apply the coating on the upper surface of the furniture board after vacuum degassing, vertically place two glass slides at both ends of the board, and then cover the two glass slides with a polytetrafluoroethylene plate, finally place a magnet on the lower surface of the furniture board, cure the entire device at 65-70°C for 2-2.5h, and repeat the above steps on the lower surface to obtain an antifouling modified furniture board;

[0008] S2: Add isocyanate and monohydroxy-terminated polydimethylsiloxane to a mixed solvent, add a catalyst and react at 75-80°C for 1-1.5 hours to obtain a prepolymer; add di(trimethylolpropane) and an antibacterial agent to N,N-dimethylformamide and stir evenly, add the prepolymer and react at 80-85°C for 60 seconds to obtain an antibacterial coating; pour the antibacterial coating on the surface of the antifouling modified furniture board, evaporate the solvent at room temperature and then place it at 130-135°C for curing for 2-2.5 hours to obtain an antibacterial and antifouling furniture board.

[0009] Furthermore, the preparation method of the graphene-modified iron-doped nano-titanium dioxide comprises the following steps:

[0010] Add hexadecylamine and potassium chloride solution to ethanol and stir evenly, add ferric chloride hexahydrate and isopropyl titanate in turn and stir evenly, let stand, filter, wash and dry to obtain an intermediate; add the intermediate to ethanol and disperse evenly, add 3-aminopropyltrimethoxysilane and reflux for 4-5 hours, wash and dry to obtain iron-doped titanium dioxide; add iron-doped titanium dioxide to graphene oxide dispersion and disperse evenly, filter and dry to obtain a composite powder; add the composite powder to an ethanol solution, place it in a reactor at 180-190°C to react for 16-18 hours, filter, dry, and then calcine at 400°C in an argon atmosphere for 2-2.5 hours to obtain graphene-modified iron-doped nano-titanium dioxide.

[0011] Furthermore, the mass ratio of the ferric chloride hexahydrate: isopropyl titanate: hexadecylamine is (0.005-0.02):(8.8-9):2.65; the concentration of potassium chloride is 0.1 mol / L; the mass ratio of the intermediate: 3-aminopropyltrimethoxysilane is (0.4-0.8):(2-4); the concentration of the graphene oxide dispersion is 5-10 mg / mL; the mass ratio of iron-doped titanium dioxide: graphene oxide dispersion is (0.4-0.5):(15-20).

[0012] Furthermore, the two glass slides are 100-400 μm above the surface of the plate; the distance between the polytetrafluoroethylene plate and the surface of the plate is 100-400 μm; the length of the two glass slides above the surface of the plate is the same as the distance between the polytetrafluoroethylene plate and the surface of the plate.

[0013] Furthermore, when the plate is placed, its surface is arranged perpendicular to the direction of the magnetic flux lines, and the direction of the magnetic field is perpendicular to the surface of the plate.

[0014] Furthermore, the thickness of the glass slide is 400 μm; the magnet is a neodymium magnet, and the magnetic field strength is 3000-5000 GS.

[0015] Furthermore, the coating thickness is 20 μm.

[0016] Furthermore, the mass ratio of the dihydroxy-terminated polydimethylsiloxane to the graphene-modified iron-doped nano-titanium dioxide is 1:(7-9).

[0017] Furthermore, the isocyanate is hexamethylene diisocyanate trimer; the mixed solvent is a mixture of butanone and propylene glycol methyl ether acetate, and the mass ratio of butanone:propylene glycol methyl ether acetate is 1.5:2; the antibacterial agent is hydroxyethyl hexahydrotriazine and triazole antibacterial agent, and the mass ratio of hydroxyethyl hexahydrotriazine:triazole antibacterial agent is (0.4-0.6):(0.4-0.6); the catalyst is dibutyltin dilaurate; the antibacterial coating is poured on the surface of the plate with a thickness of 20-50μm.

[0018] Furthermore, the mass ratio of isocyanate: monohydroxy-terminated polydimethylsiloxane is (2-2.5):(0.08-0.09); the mass ratio of prepolymer: di(trimethylolpropane) is 10:1; and the mass of the antibacterial agent is 5-8wt% of the total mass of the prepolymer and di(trimethylolpropane).

[0019] Furthermore, the method for preparing the triazole antibacterial agent comprises the following steps:

[0020] Aluminum trichloride and 1,3-dichlorobenzene are stirred evenly, then added to chloroacetyl chloride and reacted at 50-55°C for 2-2.5 hours, purified to obtain substance A; 1,2,4-triazole and triethylamine are added to ethyl acetate and heated to reflux for 1-1.5 hours, substance A is added and refluxed for 2-2.5 hours, purified to obtain substance B; substance B, trimethyl sulfoxide iodide and hexadecyl ammonium bromide are added to toluene-sodium hydroxide solution and reacted at 60-65°C for 3-3.5 hours, purified to obtain substance C; substance C is added to N,N-dimethylformamide and stirred evenly, p-methylphenol and potassium carbonate are added to react at 90-95°C, purified to obtain a triazole antibacterial agent.

[0021] Furthermore, the mass ratio of the aluminum chloride: 1,3-dichlorobenzene: chloroacetyl chloride is 22.5:14.7:13.5; the mass ratio of the 1,2,4-triazole: triethylamine: substance A is 15.1:7.6:21.3; the mass ratio of the substance B: trimethyl sulfoxide iodide: hexadecyl ammonium bromide is 5.6:4.8:0.21; the mass ratio of the substance C: p-methylphenol: potassium carbonate is 5.2:2.7:8.1.

[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0023] The present invention uses iron-doped titanium dioxide as a matrix, and prepares graphene-modified iron-doped titanium dioxide by combining a hydrothermal reaction with a sol-gel method; firstly, the iron ions inside the graphene-modified iron-doped titanium dioxide can serve as a "catcher" for electrons and holes, and are reduced to ferrous ions through photoelectron capture and then oxidized to ferric ions through oxygen, which is beneficial to the separation of electrons and holes, thereby improving the photocatalytic activity; secondly, the graphene loaded on the surface of the graphene-modified iron-doped titanium dioxide can adsorb pollutants, dyes, bacteria and other substances through the Π-Π effect, and achieve the antibacterial and antifouling effect through photocatalytic degradation, and the iron ions and graphene greatly improve the titanium dioxide Catalytic degradation performance and adsorption performance; finally, titanium dioxide is made magnetic by iron doping. Under the action of magnetic ions in the magnetic field, graphene-modified iron-doped titanium dioxide polymerizes on the surface of the plate along the direction of the magnetic flux lines, and gathers upward along the direction of the magnetic flux lines under the action of dihydroxy-terminated polydimethylsiloxane. When it reaches the polytetrafluoroethylene plate, it diffuses to the surroundings, and finally forms a microstructure with uniform spacing. This surface uniform rough structure presents concave angle characteristics. These evenly distributed concave angles can generate a combined force to lift it upward, which can prevent low surface tension pollutant droplets from penetrating into the structure and reaching the surface of the plate, achieving the effects of anti-fouling, waterproofing, and oil repellency. Even if a small amount of pollutants penetrate into the structure, they can be degraded through the photocatalytic activity of the microstructure itself, further enhancing the antibacterial and antifouling properties of the plate.

[0024] The present invention prepares an antibacterial coating for antibacterial and anticorrosive (white rot fungi, brown rot fungi, and mildew) treatment of plant boards by grafting antibacterial agent hydroxyethyl hexahydro-s-triazine into a polymer system and then blending the mixture with a triazole antibacterial agent for tree and plant boards; the antibacterial coating is poured and cured on the surface of the board to form an antibacterial coating; on the one hand, the microstructure formed by graphene-modified iron-doped titanium dioxide is structurally reinforced so that it can be further tightly combined with the board, thereby greatly improving the wear resistance of the microstructure and improving the service life; at the same time, due to the high degree of control, the columnar microstructure can still contact the pollution source liquid at the first time and still has good anti-fouling, waterproof and oil-proof effects; on the other hand, the antibacterial agent hydroxyethyl hexahydro-s-triazine provides a large number of hydroxyl cross-linking points for polymer cross-linking grafting, thereby greatly improving the cross-linking density; the low surface energy monohydroxyl-terminated polydimethylsiloxane further enhances the antibacterial and antifouling properties of the coating, thereby having excellent anti-bacterial adhesion properties. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the following examples, graphene oxide was purchased from TCI (Shanghai) Chemical Industry Development Co., Ltd., product number: G0443; dihydroxy-terminated polydimethylsiloxane was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.; monohydroxy-terminated polydimethylsiloxane was purchased from Foshan Silicification Trading Co., Ltd.; hexamethylene diisocyanate trimer was purchased from Bayer MaterialScience (China) Co., Ltd., NCO%=16.5±0.5%; the remaining raw materials were commercially available.

[0027] The preparation method of the triazole antibacterial agent comprises the following steps:

[0028] 22.5g aluminum chloride and 14.7g 1,3-dichlorobenzene were stirred evenly, then added to 13.5g chloroacetyl chloride and reacted at 50°C for 2h. Water was added under ice bath, and it was recrystallized with petroleum ether and ethyl acetate solution to obtain substance A. 15.1g 1,2,4-triazole and 7.6g triethylamine were added to 100mL ethyl acetate and heated to reflux for 1h. 21.3g substance A and 40mL ethyl acetate were added and refluxed for 2-2.5h. The filtrate was filtered and washed with The product was washed, dried, the solvent was removed, and recrystallized to obtain substance B; 5.6 g of substance B, 4.8 g of trimethylsulfoxide iodide, and 0.21 g of hexadecylammonium bromide were added to 40 mL of toluene-20% w / w sodium hydroxide solution and reacted at 60°C for 3 h, and purified to obtain substance C; 5.2 g of substance C was added to N,N-dimethylformamide and stirred evenly, and 2.7 g of p-methylphenol and 8.1 g of potassium carbonate were added to react at 90°C, purified, and a triazole antibacterial agent was obtained.

[0029] Embodiment 1: A process for producing an antibacterial and antifouling furniture board: S1: Add 2.65g of hexadecylamine and 2mL of 0.1molL potassium chloride solution to ethanol and stir evenly, add 5mg of ferric chloride hexahydrate and 8.8g of isopropyl titanate in turn and stir evenly, let stand, filter, wash, and dry to obtain an intermediate; add 0.4g of the intermediate to 200mL of ethanol and disperse evenly, add 2g of 3-aminopropyltrimethoxysilane and reflux for 4h, wash, and dry to obtain iron-doped titanium dioxide; add 0.4g of iron-doped titanium dioxide to 20mL of 5mg / mL graphene oxide dispersion and disperse evenly, filter, and dry to obtain a composite powder; add the composite powder to an ethanol solution, place it in a reactor at 180°C for reaction for 16h, filter, dry, and then calcine at 400°C in an argon atmosphere for 2h to obtain graphene-modified iron-doped nano-titanium dioxide;

[0030] S2: 10g of dihydroxy-terminated polydimethylsiloxane and 70g of graphene-modified iron-doped nano-titanium dioxide were mixed evenly to obtain an antifouling coating; after vacuum degassing, the coating was applied on the upper surface of the furniture board with a thickness of 20μm, and two glass slides were placed vertically at both ends of the board, 100μm above the board surface; then a polytetrafluoroethylene plate was covered on the two glass slides, and the distance between the polytetrafluoroethylene plate and the board surface was 100μm; finally, a Ru magnet was placed on the lower surface of the furniture board, and the entire device was cured at 65°C for 2h, and the above steps were repeated on the lower surface to obtain an antifouling modified furniture board;

[0031] S3: Add 2g of hexamethylene diisocyanate trimer and 0.08g of monohydroxy-terminated polydimethylsiloxane to a mixed solution of 1.5g of butanone and 2g of propylene glycol methyl ether acetate, add 0.01g of dibutyltin dilaurate and react at 75°C for 1h to obtain a prepolymer; add 1g of di(trimethylolpropane), 0.275g of hydroxyethylhexahydrotriazine and 0.275g of triazole antibacterial agent to N,N-dimethylformamide and stir evenly, add 10g of prepolymer and react at 80°C for 60s to obtain an antibacterial coating; pour the antibacterial coating on the surface of the antifouling modified furniture board with a pouring thickness of 20μm; evaporate the solvent at room temperature and then place it at 130°C for curing for 2h to obtain an antibacterial and antifouling furniture board.

[0032] Embodiment 2: A process for producing an antibacterial and antifouling furniture board: S1: Add 2.65g of hexadecylamine and 2mL of 0.1molL potassium chloride solution to ethanol and stir evenly, add 10mg of ferric chloride hexahydrate and 8.8g of isopropyl titanate in turn and stir evenly, let stand, filter, wash, and dry to obtain an intermediate; add 0.4g of the intermediate to 200mL of ethanol and disperse evenly, add 2g of 3-aminopropyltrimethoxysilane and reflux for 4h, wash, and dry to obtain iron-doped titanium dioxide; add 0.4g of iron-doped titanium dioxide to 20mL of 5mg / mL graphene oxide dispersion and disperse evenly, filter, and dry to obtain a composite powder; add the composite powder to an ethanol solution, place it in a reactor at 180°C for reaction for 16h, filter, dry, and then calcine at 400°C in an argon atmosphere for 2h to obtain graphene-modified iron-doped nano-titanium dioxide;

[0033] S2: 10g of dihydroxy-terminated polydimethylsiloxane and 80g of graphene-modified iron-doped nano-titanium dioxide are mixed evenly to obtain an antifouling coating; after vacuum degassing, the coating is applied on the upper surface of the furniture board with a thickness of 20μm, and two glass slides are placed vertically at both ends of the board, 100μm above the board surface; then a polytetrafluoroethylene plate is covered on the two glass slides, and the distance between the polytetrafluoroethylene plate and the board surface is 100μm; finally, a Ru magnet is placed on the lower surface of the furniture board, the entire device is cured at 65°C for 2h, and the above steps are repeated on the lower surface to obtain an antifouling modified furniture board;

[0034] S3: Add 2g of hexamethylene diisocyanate trimer and 0.08g of monohydroxy-terminated polydimethylsiloxane to a mixed solution of 1.5g of butanone and 2g of propylene glycol methyl ether acetate, add 0.01g of dibutyltin dilaurate and react at 75°C for 1h to obtain a prepolymer; add 1g of di(trimethylolpropane), 0.44g of hydroxyethylhexahydrotriazine and 0.44g of triazole antibacterial agent to N,N-dimethylformamide and stir evenly, add 10g of prepolymer and react at 80°C for 60s to obtain an antibacterial coating; pour the antibacterial coating on the surface of the antifouling modified furniture board with a pouring thickness of 20μm; evaporate the solvent at room temperature and then place it at 130°C for 2h to obtain antibacterial and antifouling furniture board.

[0035] Embodiment 3: A process for producing an antibacterial and antifouling furniture board: S1: Add 2.65g of hexadecylamine and 2mL of 0.1molL potassium chloride solution to ethanol and stir evenly, add 20mg of ferric chloride hexahydrate and 8.8g of isopropyl titanate in turn and stir evenly, let stand, filter, wash, and dry to obtain an intermediate; add 0.4g of the intermediate to 200mL of ethanol and disperse evenly, add 2g of 3-aminopropyltrimethoxysilane and reflux for 4h, wash, and dry to obtain iron-doped titanium dioxide; add 0.4g of iron-doped titanium dioxide to 20mL of 10mg / mL graphene oxide dispersion and disperse evenly, filter, and dry to obtain a composite powder; add the composite powder to an ethanol solution, place it in a reactor at 180°C for reaction for 16h, filter, dry, and then calcine at 400°C in an argon atmosphere for 2h to obtain graphene-modified iron-doped nano-titanium dioxide;

[0036] S2: 10g of dihydroxy-terminated polydimethylsiloxane and 90g of graphene-modified iron-doped nano-titanium dioxide were mixed evenly to obtain an antifouling coating; after vacuum degassing, the coating was applied on the upper surface of the furniture board with a thickness of 20μm, and two glass slides were placed vertically at both ends of the board, 100μm above the board surface; then a polytetrafluoroethylene plate was covered on the two glass slides, and the distance between the polytetrafluoroethylene plate and the board surface was 100μm; finally, a Ru magnet was placed on the lower surface of the furniture board, the entire device was cured at 65°C for 2h, and the above steps were repeated on the lower surface to obtain an antifouling modified furniture board;

[0037] S3: Add 2g of hexamethylene diisocyanate trimer and 0.08g of monohydroxy-terminated polydimethylsiloxane to a mixed solution of 1.5g of butanone and 2g of propylene glycol methyl ether acetate, add 0.01g of dibutyltin dilaurate and react at 75°C for 1h to obtain a prepolymer; add 1g of di(trimethylolpropane), 0.352g of hydroxyethylhexahydrotriazine and 0.528g of triazole antibacterial agent to N,N-dimethylformamide and stir evenly, add 10g of prepolymer and react at 80°C for 60s to obtain an antibacterial coating; pour the antibacterial coating on the surface of the antifouling modified furniture board with a pouring thickness of 20μm; evaporate the solvent at room temperature and then place it at 130°C for curing for 2h to obtain an antibacterial and antifouling furniture board.

[0038] Comparative Example 1: A process for preparing an antibacterial and antifouling furniture board: S1: 10 g of dihydroxy-terminated polydimethylsiloxane and 70 g of nano-ferroferric oxide are mixed evenly to obtain an antifouling coating; after vacuum degassing, the coating is applied on the upper surface of the furniture board to a thickness of 20 μm, and two glass slides are vertically placed at both ends of the board, 100 μm above the board surface; a polytetrafluoroethylene plate is then covered on the two glass slides, and the distance between the polytetrafluoroethylene plate and the board surface is 100 μm; finally, a ruthenium magnet is placed on the lower surface of the furniture board, the entire device is cured at 65°C for 2 hours, and the above steps are repeated on the lower surface to obtain an antifouling modified furniture board;

[0039] S3: Add 2g of hexamethylene diisocyanate trimer and 0.08g of monohydroxy-terminated polydimethylsiloxane to a mixed solution of 1.5g of butanone and 2g of propylene glycol methyl ether acetate, add 0.01g of dibutyltin dilaurate and react at 75°C for 1h to obtain a prepolymer; add 1g of di(trimethylolpropane), 0.275g of hydroxyethylhexahydrotriazine and 0.275g of triazole antibacterial agent to N,N-dimethylformamide and stir evenly, add 10g of prepolymer and react at 80°C for 60s to obtain an antibacterial coating; pour the antibacterial coating on the surface of the antifouling modified furniture board with a pouring thickness of 20μm; evaporate the solvent at room temperature and then place it at 130°C for curing for 2h to obtain an antibacterial and antifouling furniture board.

[0040] Comparative Example 2: A process for producing an antibacterial and antifouling furniture board: S1: Add 2.65g of hexadecylamine and 2mL of 0.1molL potassium chloride solution to ethanol and stir evenly, add 5mg of ferric chloride hexahydrate and 8.8g of isopropyl titanate in turn and stir evenly, let stand, filter, wash, and dry to obtain an intermediate; add 0.4g of the intermediate to 200mL of ethanol and disperse evenly, add 2g of 3-aminopropyltrimethoxysilane and reflux for 4h, wash, and dry to obtain iron-doped titanium dioxide; add 0.4g of iron-doped titanium dioxide to 20mL of 5mg / mL graphene oxide dispersion and disperse evenly, filter, and dry to obtain a composite powder; add the composite powder to an ethanol solution, place it in a reactor at 180°C for reaction for 16h, filter, dry, and then calcine at 400°C in an argon atmosphere for 2h to obtain graphene-modified iron-doped nano-titanium dioxide;

[0041] S2: 10g of dihydroxy-terminated polydimethylsiloxane and 70g of graphene-modified iron-doped nano-titanium dioxide were mixed evenly to obtain an antifouling coating; after vacuum degassing, it was coated on the upper surface of the furniture board with a thickness of 20μm, and two glass slides were placed vertically at both ends of the board, 10μm above the board surface; then a polytetrafluoroethylene plate was covered on the two glass slides, and the distance between the polytetrafluoroethylene plate and the board surface was 10μm; finally, a Ru magnet was placed on the lower surface of the furniture board, and the entire device was cured at 65°C for 2h, and the above steps were repeated on the lower surface to obtain an antifouling modified furniture board;

[0042] S3: Add 2g of hexamethylene diisocyanate trimer and 0.08g of monohydroxy-terminated polydimethylsiloxane to a mixed solution of 1.5g of butanone and 2g of propylene glycol methyl ether acetate, add 0.01g of dibutyltin dilaurate and react at 75°C for 1h to obtain a prepolymer; add 1g of di(trimethylolpropane), 0.275g of hydroxyethyl hexahydrotriazine and 0.275g of triazole antibacterial agent to N,N-dimethylformamide and stir evenly, add 10g of prepolymer and react at 80°C for 60s to obtain an antibacterial coating; pour the antibacterial coating on the surface of antifouling modified furniture board with a pouring thickness of 20μm; evaporate the solvent at room temperature and then place it at 130°C for 2h to obtain an antibacterial and antifouling furniture board

[0043] Comparative Example 3: A process for producing an antibacterial and antifouling furniture board: S1: Add 2.65g of hexadecylamine and 2mL of 0.1molL potassium chloride solution to ethanol and stir evenly, add 5mg of ferric chloride hexahydrate and 8.8g of isopropyl titanate in turn and stir evenly, let stand, filter, wash, and dry to obtain an intermediate; add 0.4g of the intermediate to 200mL of ethanol and disperse evenly, add 2g of 3-aminopropyltrimethoxysilane and reflux for 4h, wash, and dry to obtain iron-doped titanium dioxide;

[0044] S2: 10g of dihydroxy-terminated polydimethylsiloxane and 70g of iron-doped nano-titanium dioxide are mixed evenly to obtain an antifouling coating; after vacuum degassing, it is coated on the upper surface of the furniture board with a thickness of 20μm, and two glass slides are placed vertically at both ends of the board, 100μm above the board surface; then a polytetrafluoroethylene plate is covered on the two glass slides, and the distance between the polytetrafluoroethylene plate and the board surface is 100μm; finally, a Ru magnet is placed on the lower surface of the furniture board, the entire device is cured at 65°C for 2h, and the above steps are repeated on the lower surface to obtain an antifouling modified furniture board;

[0045] S3: Add 2g of hexamethylene diisocyanate trimer and 0.08g of monohydroxy-terminated polydimethylsiloxane to a mixed solution of 1.5g of butanone and 2g of propylene glycol methyl ether acetate, add 0.01g of dibutyltin dilaurate and react at 75°C for 1h to obtain a prepolymer; add 1g of di(trimethylolpropane), 0.275g of hydroxyethylhexahydrotriazine and 0.275g of triazole antibacterial agent to N,N-dimethylformamide and stir evenly, add 10g of prepolymer and react at 80°C for 60s to obtain an antibacterial coating; pour the antibacterial coating on the surface of the antifouling modified furniture board with a pouring thickness of 20μm; evaporate the solvent at room temperature and then place it at 130°C for curing for 2h to obtain an antibacterial and antifouling furniture board.

[0046] Comparative Example 4: A process for producing an antibacterial and antifouling furniture board: S1: Add 2.65g of hexadecylamine and 2mL of 0.1molL potassium chloride solution to ethanol and stir evenly, add 5mg of ferric chloride hexahydrate and 8.8g of isopropyl titanate in turn and stir evenly, let stand, filter, wash, and dry to obtain an intermediate; add 0.4g of the intermediate to 200mL of ethanol and disperse evenly, add 2g of 3-aminopropyltrimethoxysilane and reflux for 4h, wash, and dry to obtain iron-doped titanium dioxide; add 0.4g of iron-doped titanium dioxide to 20mL of 5mg / mL graphene oxide dispersion and disperse evenly, filter, and dry to obtain a composite powder; add the composite powder to the ethanol solution, place it in a reactor at 180°C for reaction for 16h, filter, dry, and then calcine at 400°C in an argon atmosphere for 2h to obtain graphene-modified iron-doped nano-titanium dioxide;

[0047] S2: Mix 10g of dihydroxy-terminated polydimethylsiloxane and 70g of graphene-modified iron-doped nano-titanium dioxide evenly to obtain an antifouling coating; apply it on the upper surface of the furniture board after vacuum degassing with a thickness of 20μm, and place two glass slides vertically at both ends of the board, 100μm above the board surface; then cover the two glass slides with a polytetrafluoroethylene plate, and the distance between the polytetrafluoroethylene plate and the board surface is 100μm; finally, place a Ru magnet on the lower surface of the furniture board, cure the entire device at 65°C for 2h, repeat the above steps on the lower surface to obtain an antibacterial and antifouling furniture board.

[0048] Test: Contact angle and rolling angle test: At room temperature, use a contact angle meter to analyze the wettability of various probe liquids on the surface of furniture panels; use 500-grit sandpaper with a width of 50 mm to move the surface of the furniture panels for 10 cm under a force of 15 N, and use the contact angle meter again to analyze the wettability of various probe liquids on the surface of furniture panels;

[0049] Antibacterial performance test: After the surface of the feed wood in the soil culture medium in the glass container is covered with hyphae, the furniture boards are sterilized and placed in the glass container under sterile conditions. They are placed in an environment with a relative temperature of 25°C and a relative humidity of 80% and cultured for 3 weeks. The quality of the furniture boards before and after is compared, and the quality loss rate is calculated; quality loss rate = (quality before the board is placed - quality after the board is placed) / quality before the board is placed.

[0050]

[0051] Conclusion: The furniture boards prepared in Examples 1-3 have excellent antibacterial and antifouling properties; in Comparative Example 1, nano-ferroferric oxide is used instead of graphene-modified iron-doped nano-titanium dioxide, which reduces the degradation ability and the adsorption performance, resulting in a decrease in antibacterial performance; in Comparative Example 2, the columnar microstructure formed by graphene-modified iron-doped nano-titanium dioxide is too short, resulting in a decrease in antibacterial performance; in Comparative Example 3, the iron-doped nano-titanium dioxide is not further modified with graphene, which reduces the antifouling and antibacterial performance; in Comparative Example 4, a polymer is not used to prepare an antibacterial coating to strengthen the columnar microstructure, so that the structure is damaged after friction, and the antifouling and antibacterial performance is reduced.

[0052] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for producing antibacterial and antifouling furniture board, characterized in that: The following steps are involved: S1: Mix dihydroxy-terminated polydimethylsiloxane and graphene-modified iron-doped nano-titanium dioxide evenly to obtain an antifouling coating; apply the coating on the upper surface of the furniture board after vacuum degassing, vertically place two glass slides at both ends of the board, and then cover the two glass slides with a polytetrafluoroethylene plate, finally place a magnet on the lower surface of the furniture board, cure the entire device at 65-70°C for 2-2.5h, and repeat the above steps on the lower surface to obtain an antifouling modified furniture board; S2: adding isocyanate and monohydroxy-terminated polydimethylsiloxane to a mixed solvent, adding a catalyst and reacting at 75-80°C for 1-1.5h to obtain a prepolymer; adding di(trimethylolpropane) and an antibacterial agent to N,N-dimethylformamide and stirring evenly, adding the prepolymer and reacting at 80-85°C for 60s to obtain an antibacterial coating; pouring the antibacterial coating on the surface of the antifouling modified furniture board, evaporating the solvent at room temperature and then curing at 130-135°C for 2-2.5h to obtain an antibacterial and antifouling furniture board; The length of the two glass slides above the surface of the plate is 100-400 μm; the distance between the polytetrafluoroethylene plate and the surface of the plate is 100-400 μm; the length of the two glass slides above the surface of the plate is the same as the distance between the polytetrafluoroethylene plate and the surface of the plate; The mass ratio of the dihydroxy-terminated polydimethylsiloxane to the graphene-modified iron-doped nano-titanium dioxide is 1:(7-9); The isocyanate is hexamethylene diisocyanate trimer; the mixed solvent is a mixture of butanone and propylene glycol methyl ether acetate, and the mass ratio of butanone to propylene glycol methyl ether acetate is 1.5:2; the antibacterial agent is hydroxyethyl hexahydro-s-triazine and triazole antibacterial agent, and the mass ratio of hydroxyethyl hexahydro-s-triazine to triazole antibacterial agent is (0.4-0.6):(0.4-0.6); the catalyst is dibutyltin dilaurate; the antibacterial coating is poured on the surface of the plate with a thickness of 20-50 μm; The mass ratio of isocyanate: monohydroxy-terminated polydimethylsiloxane is (2-2.5):(0.08-0.09); the mass ratio of prepolymer: di(trimethylolpropane) is 10:1; and the mass of the antibacterial agent is 5-8wt% of the total mass of the prepolymer and di(trimethylolpropane).

2. The process for producing an antibacterial and antifouling furniture board according to claim 1, characterized in that: The preparation method of the graphene-modified iron-doped nano-titanium dioxide comprises the following steps: Add hexadecylamine and potassium chloride solution to ethanol and stir evenly, add ferric chloride hexahydrate and isopropyl titanate in turn and stir evenly, let stand, filter, wash and dry to obtain an intermediate; add the intermediate to ethanol and disperse evenly, add 3-aminopropyltrimethoxysilane and reflux for 4-5 hours, wash and dry to obtain iron-doped titanium dioxide; add iron-doped titanium dioxide to graphene oxide dispersion and disperse evenly, filter and dry to obtain a composite powder; add the composite powder to an ethanol solution, place it in a reactor at 180-190°C to react for 16-18 hours, filter, dry, and then calcine at 400°C in an argon atmosphere for 2-2.5 hours to obtain graphene-modified iron-doped nano-titanium dioxide.

3. The process for producing an antibacterial and antifouling furniture board according to claim 2, characterized in that: The mass ratio of the ferric chloride hexahydrate: isopropyl titanate: hexadecylamine is (0.005-0.02):(8.8-9):2.65; the concentration of potassium chloride is 0.1 mol / L; the mass ratio of the intermediate: 3-aminopropyltrimethoxysilane is (0.4-0.8):(2-4); the concentration of the graphene oxide dispersion is 5-10 mg / mL; the mass ratio of iron-doped titanium dioxide: graphene oxide dispersion is (0.4-0.5):(15-20).

4. The process for producing an antibacterial and antifouling furniture board according to claim 1, characterized in that: The method for preparing the triazole antibacterial agent comprises the following steps: Aluminum trichloride and 1,3-dichlorobenzene are stirred evenly, then added to chloroacetyl chloride and reacted at 50-55°C for 2-2.5 hours, purified to obtain substance A; 1,2,4-triazole and triethylamine are added to ethyl acetate and heated to reflux for 1-1.5 hours, substance A is added and refluxed for 2-2.5 hours, purified to obtain substance B; substance B, trimethyl sulfoxide iodide and hexadecyl ammonium bromide are added to toluene-sodium hydroxide solution and reacted at 60-65°C for 3-3.5 hours, purified to obtain substance C; substance C is added to N,N-dimethylformamide and stirred evenly, p-methylphenol and potassium carbonate are added to react at 90-95°C, purified to obtain a triazole antibacterial agent.

5. The process for producing an antibacterial and antifouling furniture board according to claim 4, characterized in that: The mass ratio of the aluminum chloride: 1,3-dichlorobenzene: chloroacetyl chloride is 22.5:14.7:13.5; the mass ratio of the 1,2,4-triazole: triethylamine: substance A is 15.1:7.6:21.3; the mass ratio of substance B: trimethyl sulfoxide iodide: hexadecyl ammonium bromide is 5.6:4.8:0.21; the mass ratio of substance C: p-methylphenol: potassium carbonate is 5.2:2.7:8.

1.

6. The furniture board prepared according to the production process of an antibacterial and antifouling furniture board according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Graphene-iron ion modified TiO2 photocatalyst composite material and preparation method thereof

    CN104588019A

  • Polyurethane coating and application thereof

    CN114149737A

  • Coating agent containing an antibacterial catalyst and method for producing the same

    JP6154036B1

  • Apparatus with waterproofing, ice protection and antifouling function

    KR1020210079834A

  • Articles comprising durable water repellent, icephobic and / or biocidal coatings

    US20210017399A1