A processing method for matte chopped glass fiber
Through heat treatment, pickling and nano-silica impregnation treatment, the problem of glass fiber shines is solved, and the gloss softness and shielding performance is improved, suitable for protection against mattressing and stealth camouflage.
Patent Information
- Application Number
- CN202311381269.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-10-24
AI Technical Summary
The prior art is difficult to effectively eliminate the gloss of glass fibers, resulting in uneven gloss distribution on the surface of the product, affecting the aesthetics, and is difficult to apply in protective mattress and stealth camouflage applications.
Pretreat chopped glass fibers by heat treatment and pickling, followed by coating with dodecyl trimethylammonium bromide and increasing surface roughness, followed by impregnation and hydrothermal aging using silane hydrolysate and nanosilicon dioxide, enhancing diffuse reflection on its surface.
The gloss softness of fiberglass is achieved, which enhances its scattering effect, eliminates the shiny gloss and improves the shielding performance, making it suitable for protective matting and stealth camouflage.
Smart Images

Figure CN117303755B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass fibers, and in particular relates to a processing method for matte chopped glass fibers. Background Art
[0002] Glass fiber is an inorganic fiber with a unique luster. It can be used as a decorative material. Its products have a shiny luster, strong light reflection performance, and a bright white appearance. For example, Shen Juan disclosed that glass fiber mesh is combined with translucent concrete to prepare glass fiber reinforced translucent concrete. Glass fiber is also used in landscape lighting technology. The reflective function of glass fiber is combined with optical fiber lighting to produce a variety of landscape sketches with different shapes. However, as people's needs change, sometimes they do not want such a dazzling luster. For example, semi-aromatic and glass fiber are mixed in different proportions to prepare high-performance fibers with a glossy surface. (Chemicfasern 1989, 39 / 91 (7 / 8), E99) discloses a matte glass fiber. In organic matte fibers, titanium dioxide matting agents are added to produce them, such as matte polyester. However, glass fiber is completely different. Titanium dioxide itself is a production additive component in glass, such as a crystal nucleating agent, and cannot play the role of a matte agent. The produced glass fiber still has a dazzling luster. In the past, matte glass fiber was used for insulation and weaving filter materials. However, in order to avoid strong light stimulation to human vision and give people an elegant and comfortable visual experience, the shiny luster of glass fiber itself affects the beauty of its products, causing uneven distribution of surface luster, which can cause visual differences, and shiny glass fiber products are difficult to use in protective matting and stealth camouflage purposes. At present, there are few related technologies and products of matt chopped glass fiber disclosed. As a person skilled in the art, it is urgent to develop a new processing method for matt chopped glass fiber. Summary of the invention
[0003] The purpose of the present invention is to provide a processing method for matte chopped glass fibers in view of the existing problems.
[0004] The present invention is achieved through the following technical solutions:
[0005] A processing method for matte chopped glass fibers comprises the following steps: the first step, pretreatment: heat treating the chopped glass fibers at 400-500°C for 20-30 minutes, pickling the heat-treated chopped glass fibers in a hydrochloric acid solution at 80°C for 4-5 hours, filtering after pickling, washing with clean water until the washing liquid is neutral, and then placing the chopped glass fibers in an oven at 70-80°C for 6-12 hours to obtain the pretreated chopped glass fibers; heat treatment removes the wetting agent and impurities on the surface of the chopped glass fibers. After cooling in the furnace, dodecyltrimethylammonium bromide is coated on the surface of the matte chopped glass fibers by electrostatic action to improve the surface roughness of the glass fibers.
[0006] Step 2: Add 0.8% to 1% dodecyltrimethylammonium bromide solution by mass to the stirring kettle, heat to 40 to 50°C, and stir for 20 to 30 minutes; then stop stirring, add chopped glass fibers to the stirring kettle and soak for 4 to 6 hours at a bath ratio of 1:8 to 10, filter and wash with clean water until the washing liquid is neutral, and then dry in an oven at 60 to 80°C for 6 to 12 hours to obtain cationic modified chopped glass fibers;
[0007] The surface structure of the glass fiber treated with silane hydrolyzate contains active groups such as hydroxyl groups, which are successfully and stably deposited on the surface of the glass fiber through the amphiphilic effect of the coupling agent, making the surface of the glass fiber rough;
[0008] The third step is to mix anhydrous ethanol and deionized water in a mass ratio of 8 to 9:1, add 0.5wt% to 0.7wt% of silane coupling agent thereto and stir continuously for 6 to 10 minutes to obtain a silane hydrolyzate, add 0.7wt% to 0.9wt% of nano-silicon dioxide to the silane hydrolyzate, stir for 40 to 60 minutes to obtain a mixed solution, and then take short chopped glass fibers according to a bath ratio of 1:12 to 15 and put them into the above mixed solution, immerse them for 15 to 20 minutes under stirring, filter them, perform hydrothermal aging, and then place them in an oven at 80 to 100°C for drying for 6 to 8 hours to obtain the treated short chopped glass fibers.
[0009] Chopped glass fiber yarn, also known as chopped glass fiber, is made by cutting continuous glass fiber roving into segments.
[0010] Furthermore, the first step chopped glass fibers are alkali-free chopped glass fibers with a fiber diameter of 10 μm to 13 μm and a chopped length of 3 mm to 4.5 mm.
[0011] Furthermore, the silane coupling agent in the third step is one of γ-aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane.
[0012] Furthermore, the nano silicon dioxide in the third step is 5 to 25 nm.
[0013] Furthermore, the concentration of the hydrochloric acid solution in the first step is 0.6-0.8 mol / L.
[0014] Furthermore, the hydrothermal aging in the third step is heating in 45-50° C. water for 2-3 hours.
[0015] Beneficial effects of the present invention:
[0016] The present invention discloses a processing method for treating chopped glass fibers to soften their luster, eliminate the bright luster on the surface of the chopped glass fibers, and avoid the existence of bright glittering light. This method can enhance the scattering effect of the chopped glass fibers and improve the diffuse scattering effect of light in the air. By adding silica particles, the surface of the chopped glass fibers can be made rough, thereby achieving the matte effect of the fibers. In addition, since the size of the silica particles is smaller than the wavelength of the incident light, when light energy is transferred to the silica particles, the electrons in the particles will vibrate with the propagation frequency of the photons, becoming a secondary propagation source, thereby continuously scattering light in all directions. Therefore, the chopped glass fibers after treatment have the characteristics of soft luster and strong shielding performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Attached Figure 1 It is the ultraviolet-visible diffuse reflectance spectra of the matt chopped glass fiber of Example 1 and the untreated chopped glass fiber of Comparative Example 1. DETAILED DESCRIPTION
[0018] The present invention is described below with specific examples, but is not intended to be limiting of the present invention. Example 1
[0019] Raw materials: Chopped glass fiber: brand ECS-3.0-T435N alkali-free glass fiber; silane coupling agent is Wanda NQ-55γ-aminopropyltriethoxysilane; nano silica DNS-1; Kangaite dodecyltrimethylammonium bromide.
[0020] The processing method of matte chopped glass fiber comprises the following steps: the first step, pretreatment: heat-treating the chopped glass fiber at 500°C for 30 minutes, pickling the heat-treated chopped glass fiber in a hydrochloric acid solution at 80°C for 5 hours, the concentration of the hydrochloric acid solution is 0.8 mol / L, filtering after pickling, washing with clean water until the washing liquid is neutral, and then placing the chopped glass fiber in an oven at 80°C for 12 hours to obtain the pretreated chopped glass fiber; the second step, adding a 1% by mass dodecyltrimethylammonium bromide solution into a stirring kettle, heating to 50°C, stirring for 30 minutes; then stopping stirring, adding the chopped glass fiber into the stirring kettle and immersing for 6 hours at a bath ratio of 1:10, filtering Then wash with clean water until the washing liquid is neutral, and then dry in an oven at 80°C for 12 hours to obtain cationic modified short glass fibers; the third step, mix anhydrous ethanol and deionized water in a mass ratio of 9:1, add 0.5wt% silane coupling agent thereto and stir continuously for 10 minutes to obtain a silane hydrolyzate, add 0.7wt% nano-silicon dioxide to the silane hydrolyzate, stir for 60 minutes to obtain a mixed solution, and then take the short glass fibers according to the bath ratio of 1:12 and put them into the above mixed solution, immerse them under stirring for 20 minutes, filter and perform hydrothermal aging, the hydrothermal aging is heating in 50°C water for 3 hours, and then placing in an oven at 100°C for drying for 8 hours to obtain the treated short glass fibers.
[0021] Product: Fiber diameter 10μm, short cut length 3mm, moisture content 0.10%. Short cut rate should be 97%, whiteness 87, surface matte, no shiny luster.
[0022] Comparative Example 1
[0023] Compared with Example 1, the comparative example is the chopped glass fibers in Example 1 without any treatment.
[0024] Product: Fiber diameter 10μm, short cut length 3mm, moisture content 0.10%, short cut rate should be 97%, whiteness 65, with bright luster.
[0025] According to the attached Figure 1 According to the analysis, the untreated chopped glass fiber powder will reflect light when exposed to light, and the glass fiber on the surface will show a bright luster. After treatment, the silica particles will make the glass fiber rough, and diffuse reflection will occur after the light enters, and the extinction effect is better. And this diffuse reflection will cause the light to scatter irregularly, making the surface of the glass fiber look white. The smaller the silica particles, the more reflective surfaces there are. In addition, the smaller the particle size, the denser and smoother the surface is when making whiteness measurement powder. After hydrothermal aging, the air gaps between the particles will also become smaller. Therefore, the diffuse reflection of light on the surface of the silica particles will be enhanced, resulting in a higher whiteness measurement value. By attaching Figure 1By comparing the diffuse reflectance spectra of UV-3900 ultraviolet visible light, it can be clearly seen that the diffuse reflectance effect of Example 1 is stronger, and the whiteness value measured by the whiteness meter is relatively high. From a macroscopic perspective, the whiteness of the matte glass fiber is relatively high, and the matte effect is achieved by scattering light. Example 2
[0026] Chopped glass fiber: ECS-3.0-T438G, alkali-free glass fiber; silane coupling agent is SICO-A111γ-aminopropyltrimethoxysilane; nano-silica DNS-2; PNQM-C031 dodecyltrimethylammonium bromide.
[0027] The processing method of matte chopped glass fiber comprises the following steps: the first step, pretreatment: heat treating the chopped glass fiber at 500°C for 30 minutes, pickling the heat-treated chopped glass fiber in a hydrochloric acid solution at 80°C for 5 hours, the concentration of the hydrochloric acid solution is 0.8 mol / L, filtering after pickling, washing with clean water until the washing liquid is neutral, and then placing the chopped glass fiber in an oven at 80°C for 12 hours to obtain the pretreated chopped glass fiber; the second step, adding a 1% by mass dodecyltrimethylammonium bromide solution into a stirring kettle, heating to 50°C, stirring for 30 minutes; then stopping stirring, adding the chopped glass fiber into the stirring kettle and immersing for 6 hours at a bath ratio of 1:10, and then drying for 12 hours. After filtering, wash with clean water until the washing liquid is neutral, and then dry in an oven at 80°C for 6 hours to obtain cationic modified short glass fibers; the third step, mix anhydrous ethanol and deionized water in a mass ratio of 8:1, add 0.7wt% silane coupling agent thereto and stir continuously for 10 minutes to obtain a silane hydrolyzate, add 0.7wt% nano-silicon dioxide to the silane hydrolyzate, stir for 60 minutes to obtain a mixed solution, and then take the short glass fibers according to the bath ratio of 1:15 and put them into the above mixed solution, immerse them under stirring for 20 minutes, filter and perform hydrothermal aging, the hydrothermal aging is heating in 50°C water for 3 hours, and then placing in an oven at 100°C for drying for 8 hours, that is, the treated short glass fibers are obtained.
[0028] Product: Fiber diameter 13μm, short cut length 4.5mm, moisture content 0.10%, short cut rate should be 97%, whiteness 85, surface matte, no shiny luster.
[0029] Note: Refer to GB / T1549-2008 Chemical Analysis Method for Fiber Glass; the fiber diameter shall be tested in accordance with the provisions of GB / T7690.5-2013 Test Method for Reinforced Material Yarn Part 5: Determination of Fiber Diameter of Glass Fiber; the combustible content shall be tested in accordance with the provisions of GB / T9914.2-2013 Test Method for Reinforced Products Part 2: Determination of Combustible Content of Glass Fiber; the moisture content shall be tested in accordance with the provisions of GB / T9914.1-2013 Test Method for Reinforced Products Part 1: Determination of Moisture Content; the short-cut rate shall be tested in accordance with the provisions of 6.6 of JC / T896-2002 Glass Fiber Chopped Strand; the short-cut length shall be tested in accordance with the provisions of 6.3 of JC / T896-2002 Glass Fiber Chopped Strand.
Claims
1. A processing method for matte chopped glass fibers, characterized in that: The method comprises the following steps: the first step, pretreatment: heat-treating the chopped glass fibers at 400-500°C for 20-30 minutes, acid-washing the heat-treated chopped glass fibers in a hydrochloric acid solution at 80°C for 4-5 hours, filtering after acid washing, washing with clean water until the washing liquid is neutral, and then placing the chopped glass fibers in an oven at 70-80°C for drying for 6-12 hours to obtain the pretreated chopped glass fibers, wherein the chopped glass fibers are alkali-free chopped glass fibers with a fiber diameter of 10μm-13μm and a chopped length of 3mm-4.5mm; the second step, adding a dodecyltrimethylammonium bromide solution with a mass fraction of 0.8%-1% into a stirring kettle, heating to 40-50°C, and stirring for 20-30 minutes; then stopping stirring, adding the chopped glass fibers into the stirring kettle and mixing them at a bath ratio of 1:8-1. 0 is immersed for 4 to 6 hours, filtered and washed with clean water until the washing liquid is neutral, and then dried in an oven at 60 to 80°C for 6 to 12 hours to obtain cationic modified short glass fibers; the third step is to mix anhydrous ethanol and deionized water in a mass ratio of 8 to 9:1, add 0.5wt% to 0.7wt% of silane coupling agent thereto and stir continuously for 6 to 10 minutes to obtain a silane hydrolyzate, add 0.7wt% to 0.9wt% of nano silicon dioxide to the silane hydrolyzate, stir for 40 to 60 minutes to obtain a mixed solution, and then take the short glass fibers according to the bath ratio of 1:12 to 15 and put them into the above mixed solution, immerse them for 15 to 20 minutes under stirring conditions, filter them, perform hydrothermal aging, and then place them in an oven at 80 to 100°C for drying for 6 to 8 hours to obtain the treated short glass fibers.
2. The processing method for chopped glass fibers according to claim 1, characterized in that: The silane coupling agent in the third step is one of γ-aminopropyltriethoxysilane and γ-aminopropyltrimethoxysilane.
3. The processing method for chopped glass fibers according to claim 1, characterized in that: The nano silicon dioxide in the third step is 5 to 25 nm.
4. The processing method for chopped glass fibers according to claim 1, characterized in that: The concentration of the hydrochloric acid solution in the first step is 0.6-0.8 mol / L.
5. The processing method for chopped glass fibers according to claim 1, characterized in that: The hydrothermal aging in the third step is heating in 45-50° C. water for 2-3 hours.
Citation Information
Patent Citations
Modified quartz fiber, and surface modification method thereof
CN108589273A
Preparation method of photovoltaic anti-reflection coating liquid capable of being cured at normal temperature and photovoltaic anti-reflection glass
CN113480878A
Anti-reflection film capable of being cured at normal temperature and preparation method of anti-reflection film
CN116285661A
Production process method of asphalt concrete reinforced chopped glass fiber
CN116715453A
Matte article and method for manufacturing same
JP2022008024A