A kind of developable embolic microsphere and its preparation method and application
Chemoembolization microspheres with stable development and good drug-loading properties are prepared through a polymerization reaction in which covalently modified developable molecules are combined with polyhydroxy polymers. This solves the problem of using a large amount of chemoembolization microsphere developer and achieves the development effect and Improvement of drug loading performance.
Patent Information
- Application Number
- CN202311245660.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing chemoembolization microspheres use a large amount of contrast agent during surgery and have strong side effects. Moreover, it is difficult to monitor the distribution of microspheres after the contrast agent is separated from the microspheres, which affects the evaluation of surgical effects.
By covalently modifying developable molecules on polyhydroxy polymers, and combining cross-linking agents to perform polymerization reactions to prepare microspheres, the degree of modification and uniformity of the developing molecules can be improved, the amount of developer can be reduced, and anionic modifiers can be used to enhance the drug-loading performance.
It has strong development stability and excellent development effect. It can clearly display the distribution of microspheres under X-rays, improve surgical visualization, reduce harm to patients, and improve the drug loading rate and drug loading rate of microspheres.
Smart Images

Figure CN117323459B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical materials, and in particular relates to a developable embolic microsphere and a preparation method and application thereof. Background Art
[0002] Transarterial chemoembolization (TACE) can achieve targeted drug delivery and selectively block the blood vessels supplying tumors, and is an ideal treatment for tumors (such as liver tumors, etc.). Among the many chemoembolic materials, embolic microspheres can pass through the delivery catheter and blood vessels more smoothly, reach the site that needs embolization more accurately and deeply, and greatly reduce damage to healthy parts. When using embolic microspheres for TACE surgery, the embolic microspheres need to be assisted in delivery with contrast agents, and real-time image-guided surgery is achieved through radiopaque contrast agents, which visualizes the treatment process and is conducive to judging the degree of embolism and the endpoint of surgical treatment. However, this method has the disadvantages of large amounts of contrast agents used during surgery and strong toxic side effects. In the middle and late stages of the operation, the microspheres and the contrast agent gradually separate, and it is difficult for medical staff to know the specific distribution of the microspheres, which seriously interferes with the judgment of the surgical effect. After the operation is completed, medical staff cannot judge the effect of microsphere embolism, or whether leakage or displacement occurs. Based on this, drug-loaded microspheres that can be visualized under X-rays have been developed. They can not only deliver anti-tumor drugs to the tumor area while embolizing, reducing damage to other parts, but also reduce the use of contrast agents during surgery and reduce the harm of contrast agents to patients. At the same time, the microspheres can be visualized during and after surgery, allowing doctors to better judge the distribution of microsphere embolism, which is beneficial for subsequent diagnosis and treatment arrangements.
[0003] At present, the methods of loading or modifying the developer on microspheres mainly include embedding method, adsorption method, covalent bonding method, etc. Among them, the embedding method and adsorption method only rely on physical force to load the developer, which is prone to leakage risk during production, storage, use, etc. The covalent bonding method usually prepares microspheres first, and then connects the iodine-containing compound to the microspheres in the form of covalent bonds through chemical reactions to reduce the risk of developer leakage. However, this method can only achieve the development modification of the microsphere surface, and the development modification effect is poor, which affects the application effect of the developable embolic microspheres to a certain extent. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing developable embolic microspheres, and the prepared developable embolic microspheres have the characteristics of good developing effect and good application prospect.
[0005] The present invention also provides a developable embolic microsphere.
[0006] The invention also provides a chemoembolization material.
[0007] The invention also provides a medical product.
[0008] The present invention also provides the application of the above-mentioned developable embolic microspheres.
[0009] In the first aspect of the present invention, a method for preparing developable embolic microspheres is proposed, comprising the following steps: covalently modifying developable molecules on a polyhydroxy polymer, and performing a polymerization reaction with raw materials including a cross-linking agent to obtain the embolic microspheres; wherein the reaction occurring when modifying the developable molecules on the polyhydroxy polymer comprises at least one of an acetal reaction or an acetal exchange reaction.
[0010] The method for preparing developable embolic microspheres according to the embodiment of the present invention has at least the following beneficial effects:
[0011] In the present invention, the developable molecules are first covalently modified on the polyhydroxy polymer to obtain the developing intermediate, and then the microspheres are synthesized, which can improve the modification degree and uniformity of the developable molecules in the microspheres, and at the same time can ensure the various physical and chemical properties of the microspheres as embolic agents, and reduce the amount of the developer in TACE. The developable embolic microspheres in the present invention have good X-ray development effect, strong development stability, and still have excellent development effect after long-term placement, which is conducive to visual monitoring and operation during and after surgery; the various physical and chemical properties of the microspheres meet the requirements of embolic agents and have a good blocking effect on target blood vessels.
[0012] In some embodiments of the present invention, the developable embolic microspheres are developable drug-loaded embolic microspheres.
[0013] In some embodiments of the present invention, the developable molecule is an iodine-containing compound.
[0014] In some embodiments of the present invention, the developable molecule includes an iodine-containing aromatic substance containing an aldehyde group or an acetal structure.
[0015] In some embodiments of the present invention, the developable molecule includes at least one of 2,3,5-triiodobenzaldehyde, 3,5-diiodobenzaldehyde dimethyl acetal, 2,3,5-triiodophenylacetaldehyde dimethyl acetal, 2,3,5-triiodobenzamide acetaldehyde dimethyl acetal or a compound of formula I:
[0016]
[0017] Wherein, A is an iodine-substituted aromatic group; n is an integer and 10≥n≥1, R 1 and R 2 Independently selected from C 1-6 An alkyl or cycloalkyl group.
[0018] In some embodiments of the invention, 4≥n≥1.
[0019] In some embodiments of the present invention, the A is selected from phenyl substituted with iodine, or phenyl co-substituted with carboxyl and iodine.
[0020] In some embodiments of the present invention, the iodine substitution in A includes at least one of monoiodine substitution, diiodine substitution, triiodine substitution, tetraiodine substitution or pentaiodine substitution.
[0021] In some embodiments of the present invention, the carboxyl substitution in A includes at least one of monocarboxyl substitution, dicarboxyl substitution, tricarboxyl substitution or tetracarboxyl substitution.
[0022] In some embodiments of the present invention, the compound of formula I is Wherein a and b are both integers, and 3≥a≥1, 3≥b≥0.
[0023] In some embodiments of the present invention, the compound of formula I includes at least one of N-(dimethoxyethyl)-5-amino-2,4,6-triiodoisophthalic acid, N-(dimethoxyethyl)-3-amino-2,4,6-triiodobenzoic acid or N-(dimethoxyethyl)-5-amino-4,6-diiodo-1,3-phthalic acid.
[0024] Through the above implementation, the compound of formula I is used as the developable molecule, and the developable embolic microspheres obtained have good developing effect.
[0025] In some embodiments of the present invention, the polyhydroxy polymer comprises at least one of polyvinyl alcohol, gelatin, polysaccharide, polyvinyl alcohol derivative, gelatin derivative or polysaccharide derivative.
[0026] In some embodiments of the present invention, the polysaccharide includes at least one of starch, chitosan, alginate, cellulose, hyaluronic acid, cellulose derivatives or hyaluronic acid derivatives. Optionally, the cellulose derivatives include but are not limited to methylcellulose, carboxymethylcellulose, ethylcellulose, hydroxyethylcellulose, cyanoethylcellulose, hydroxypropylcellulose or hydroxypropylmethylcellulose, etc. Optionally, the hyaluronic acid derivatives include but are not limited to sodium hyaluronate, hydrolyzed hyaluronic acid, silanized hyaluronic acid or hydroxypropyltrimethylammonium chloride hyaluronic acid, etc.
[0027] In some embodiments of the present invention, the polyhydroxy polymer includes at least one of a 1,2-diol structure or a 1,3-diol structure.
[0028] In some embodiments of the present invention, the polyhydroxy polymer is soluble in an acidic system, which can further facilitate the modification of the developable molecules.
[0029] In some embodiments of the present invention, the molecular weight of the polyhydroxy polymer is comprised between 10,000 and 300,000.
[0030] In some embodiments of the present invention, the mass ratio of the polyhydroxy polymer to the developable molecule comprises 1:(0.01-1.5).
[0031] In some embodiments of the present invention, the mass ratio of the polyhydroxy polymer to the developable molecule comprises 1:(0.1-0.5).
[0032] In some embodiments of the present invention, the modification rate of the developable molecules on the polyhydroxy polymer is 60-85%.
[0033] In some embodiments of the present invention, in the preparation method, the developable molecules and the anionic modifier are modified on the polyhydroxy polymer before the polymerization reaction is carried out.
[0034] In some embodiments of the present invention, in the preparation method, the developable molecule and the anion modifier are sequentially modified on the polyhydroxy polymer, and then a polymerization reaction is carried out.
[0035] Through the above implementation, in the process of preparing embolic microspheres in the present invention, the present invention first synthesizes a developable intermediate, then modifies anionic functional groups and prepares microspheres, and the degree of modification of the developable molecules in the microspheres is higher and the distribution is more uniform; based on the modification of anionic modifiers, the microspheres have a fast drug loading speed and a large drug loading amount, which is convenient for clinical operation and has a good effect on tumor treatment; the developable embolic microspheres of the present invention can not only load anti-tumor drugs well, but also understand the microsphere tissue distribution during and after surgery, which can simultaneously achieve good treatment and visualization effects. And the experiment found that the developable molecules and anionic modifiers have a synergistic effect, and the embolic microspheres modified with developable molecules have a faster drug loading rate than the embolic microspheres without modified developable molecules.
[0036] The modification of the anionic modifier in the present invention is conducive to improving the drug loading performance of the developable embolic microspheres; and the method of first modifying the anionic modifier and then polymerizing into spheres in the present invention is conducive to the uniform modification of the anionic modifier in the microspheres to a great extent, and the modification effect is good, which is convenient for improving the drug loading performance of the developable embolic microspheres, such as drug loading rate, drug loading rate, etc. Among them, there are many ways to modify the anionic modifier, such as directly forming a covalent bond with the hydroxyl group on the polyhydroxy polymer, or modifying the polyhydroxy polymer (including the polyhydroxy polymer modified with the developable molecule) through the connection of a crosslinking agent.
[0037] In some embodiments of the present invention, the anionic modifier is modified on the polyhydroxy polymer or / and on the polyhydroxy polymer modified with the developable molecule through a covalent bond.
[0038] In some embodiments of the present invention, the reaction of modifying the polyhydroxy polymer or / and the polyhydroxy polymer modified with the developable molecule with the anion modifier comprises at least one of an acetal reaction, an acetal exchange reaction or a cross-linking reaction.
[0039] According to the above embodiment, the anion modifier is modified on the polyhydroxy polymer or the polyhydroxy polymer modified with the developable molecule by acetal reaction, acetal exchange reaction or cross-linking reaction. Optionally, the cross-linking reaction includes but is not limited to free radical reverse suspension polymerization reaction.
[0040] In some embodiments of the present invention, the anion modifier includes at least one of an organic acid containing an unsaturated functional group or a salt of an organic acid containing an unsaturated functional group.
[0041] In some embodiments of the present invention, the unsaturated functional group includes at least one of an aldehyde group, an acetal group, a ketone group or an acryloyl group.
[0042] In some embodiments of the present invention, the organic acid comprises at least one of an organic carboxylic acid, an organic sulfonic acid or an organic phosphoric acid.
[0043] In some embodiments of the present invention, the organic acid has at least one acidic group.
[0044] In some embodiments of the present invention, the anionic modifier contains at least one unsaturated functional group.
[0045] In some embodiments of the present invention, the salt of the organic acid comprises at least one of a sodium salt or a potassium salt.
[0046] In some embodiments of the present invention, the anion modifier includes at least one of an acid substance containing an aldehyde group, an acetal group or a ketone group, a salt of the acid substance, an organic acid containing an acryloyl group or a salt of an organic acid containing an acryloyl group.
[0047] In the present invention, through the above-mentioned embodiment, the anion modifier includes an acid-containing monomer, which can be used as a reaction catalyst for the developable molecule modification and / or anion modification, and can also be used as a reaction monomer, so that the reaction system is simplified, the post-processing steps of the microsphere preparation are reduced, the reaction steps are simplified, and the operation is simple. Specifically, the acid-containing monomer can provide acidic conditions at the initial stage of the developable embolic microsphere preparation step (such as the developable molecule modification stage or the anion modifier modification stage), thereby catalyzing and promoting each modification reaction and will not affect its participation in subsequent polymerization reactions, thereby reducing the use of other reagents (such as strong acids, catalysts, solvents required for reactions or post-processing).
[0048] In some embodiments of the present invention, the acid substance containing an aldehyde group, an acetal group or a ketone group includes at least one of glyoxylic acid, propionaldehyde acid or acetone dicarboxylic acid.
[0049] In some embodiments of the present invention, the organic acid containing an acryl group includes at least one of 2-acrylamido-2-methylpropanesulfonic acid, acrylic acid or acrylylglycine.
[0050] In some embodiments of the present invention, the anion modifier includes an organic acid containing an acryloyl group and a salt of an organic acid containing an acryloyl group.
[0051] In some embodiments of the present invention, the mass ratio of the organic acid containing acryl group to the salt of the organic acid containing acryl group comprises (0.5-10):1, and can be optionally (1-4):1.
[0052] Through the above implementation, the obtained developable embolic microspheres have better sphericity, better microsphere compression performance, better drug loading performance and better microsphere stability.
[0053] In some embodiments of the present invention, the mass ratio of the polyhydroxy polymer to the anionic modifier comprises 1:(0.05-8).
[0054] In some embodiments of the present invention, the mass ratio of the polyhydroxy polymer to the anionic modifier includes 1:(0.1-4), and can be optionally 1:(0.1-1).
[0055] In some embodiments of the present invention, the mass ratio of the polyhydroxy polymer, the developable molecule and the anionic modifier comprises 1:(0.01-1.5):(0.05-8).
[0056] In some embodiments of the present invention, the cross-linking agent contains a functional group.
[0057] In some embodiments of the present invention, the functional group in the cross-linking agent is selected from at least one of an aldehyde group, an acetal group or an acryloyl group.
[0058] In some embodiments of the present invention, the cross-linking agent is a multifunctional cross-linking agent.
[0059] In some embodiments of the present invention, the crosslinking agent is a bifunctional crosslinking agent, one functional group includes at least one of an aldehyde group or an acetal group, and the other functional group includes at least one of an aldehyde group, an acetal group or an acryloyl group.
[0060] In some embodiments of the present invention, the cross-linking agent includes at least one of glutaraldehyde, formaldehyde, N-(2,2-dimethoxyethyl)-2-acrylamide or N-(2,2-diethoxyethyl)-2-acrylamide.
[0061] In some embodiments of the present invention, the mass ratio of the polyhydroxy polymer to the crosslinking agent includes (0.5-200): 1. For example, it can be (100-200): 1, or (1-20): 1.
[0062] In some embodiments of the present invention, the preparation method comprises the following steps:
[0063] S1, mixing a polyhydroxy polymer, a developable molecule, an anionic modifier, a crosslinking agent and water to obtain an aqueous phase material;
[0064] S2, mixing the aqueous phase material and the oil phase material, polymerizing, and obtaining the developable embolic microspheres.
[0065] In some embodiments of the present invention, in step S1: a polyhydroxy polymer is mixed with water to obtain a polyhydroxy polymer solution, which is then mixed with a developable molecule, an anionic modifier and a cross-linking agent.
[0066] In some embodiments of the present invention, in step S1, 1 part of polyhydroxy polymer is mixed with 5-15 parts of water and heated to obtain the polyhydroxy polymer solution. Optionally, the heating temperature includes 40-100°C.
[0067] In some embodiments of the present invention, the mass ratio of the polyhydroxy polymer solution to the anionic modifier, the developable molecule and the crosslinking agent includes (6-16): (0.05-8): (0.01-1.5): (0.005-2).
[0068] In some embodiments of the present invention, when the anionic modifier includes at least one of an acid substance containing an aldehyde group, an acetal group or a ketone group or a salt of the acid substance, step S1 includes the following steps: mixing the polyhydroxy polymer solution with the developable molecule, then adding the anionic modifier and the crosslinking agent, mixing, and obtaining the aqueous phase material. Optionally, the two mixing methods in step S1 are independently selected from mixing at a temperature of T1, T1 = 20-60°C. Optionally, in the mixing step after adding the anionic modifier and the crosslinking agent, the mixing time can be 10min-6h.
[0069] In some embodiments of the present invention, when the anionic modifier includes at least one of an organic acid containing an acryloyl group or a salt of an organic acid containing an acryloyl group, step S1 includes the following steps: mixing the polyhydroxy polymer solution with a developable molecule, anionic modifier and a crosslinking agent, and then adding persulfate to obtain the aqueous phase material. Optionally, the mixing time includes but is not limited to 10 min-14 h, and the mixing temperature includes but is not limited to 20-90° C.
[0070] In some embodiments of the present invention, when the anionic modifier includes at least one of an organic acid containing an acryloyl group or a salt of an organic acid containing an acryloyl group, step S1 includes the following steps: mixing the polyhydroxy polymer solution with the developable molecule, reacting, then mixing with the anionic modifier and the cross-linking agent, and then adding persulfate to obtain the aqueous phase material.
[0071] In some embodiments of the present invention, the mixing and reaction step with the developable molecules includes reacting at a temperature T2, the reaction temperature T2 includes 40-90°C, and the reaction time includes 7-14h. In some embodiments of the present invention, the mixing method with the anionic modifier and the crosslinking agent includes mixing at a temperature T3, T3 includes 20-60°C, and the mixing time includes 2-8h. Optionally, the mixing method can be stirring.
[0072] In some embodiments of the present invention, the persulfate includes at least one of potassium persulfate, sodium persulfate or ammonium persulfate. The addition of persulfate further promotes the modification reaction of the anion modifier, which is beneficial to improving the drug loading performance of the developable embolic microspheres.
[0073] In some embodiments of the present invention, the mass ratio of the anion modifier to the persulfate comprises 1:(0.001-0.1).
[0074] In some embodiments of the present invention, the preparation method further comprises the preparation of an oil phase material, specifically comprising: heating and mixing a cellulose acetate butyrate substance with an organic solvent I to obtain the oil phase material. Optionally, the heating temperature is 30-80°C.
[0075] In some embodiments of the present invention, the organic solvent I comprises at least one of butyl acetate, ethyl acetate or propyl acetate.
[0076] In some embodiments of the present invention, the mass ratio of the cellulose acetate butyrate substance to the organic solvent I is 1:(20-80).
[0077] In some embodiments of the present invention, step S2 includes the following steps: mixing the aqueous phase material with the oil phase material, stirring to form water-in-oil droplets, heating to polymerize, and washing to obtain the developable embolic microspheres.
[0078] In some embodiments of the present invention, in step S2, the temperature of the heating polymerization is 50-90° C.; and / or the time of the heating polymerization is 3-8 hours.
[0079] In some embodiments of the present invention, in step S2, after the polymerization reaction is completed, washing is performed using an organic solvent II, a buffer solution, and pure water in sequence.
[0080] In some embodiments of the present invention, the organic solvent II comprises at least one of butyl acetate, ethanol or acetone.
[0081] In some embodiments of the present invention, the buffer solution includes at least one of a PBS buffer solution, a sodium bicarbonate-sodium carbonate buffer solution, or a disodium hydrogen phosphate-sodium hydrogen phosphate buffer solution.
[0082] In some embodiments of the present invention, in step S2, after washing, the microspheres are sieved to obtain developable embolic microspheres of various particle sizes.
[0083] In some embodiments of the present invention, the preparation method further comprises step S3: mixing the developable embolic microspheres prepared in step S2 with active ingredients to obtain developable embolic microspheres loaded with the active ingredients.
[0084] In some embodiments of the present invention, the active ingredients include, but are not limited to, one or more of drugs, polypeptides or protein active factors, etc.
[0085] In some embodiments of the present invention, the drug includes but is not limited to one or more of fluorouracil, cisplatin, mitomycin, gemcitabine, capecitabine, irinotecan, sorafenib, sunitinib, bevacizumab, erlotinib, daunorubicin, cyclophosphamide, doxorubicin, vincristine, mitoxantrone, methotrexate, teniposide, etoposide, gefitinib, afatinib, Herceptin monoclonal antibody or lapatinib.
[0086] In some embodiments of the present invention, step S3 comprises: swelling the developable embolic microspheres obtained in step S2 with a swelling agent, and then mixing with active ingredients to obtain developable embolic microspheres loaded with the active ingredients.
[0087] In some embodiments of the present invention, the swelling agent includes but is not limited to physiological saline.
[0088] In some embodiments of the present invention, step S3 comprises: after swelling the developable embolic microspheres obtained in step S2 with a swelling agent, mixing with a doxorubicin hydrochloride solution to obtain developable embolic microspheres loaded with the active ingredient. Optionally, the doxorubicin hydrochloride solution comprises an aqueous solution of doxorubicin hydrochloride. Optionally, the amount ratio of the developable embolic microspheres to the aqueous solution of doxorubicin hydrochloride comprises 1mL:(10-50)mg. Optionally, the concentration of doxorubicin hydrochloride in the aqueous solution of doxorubicin hydrochloride comprises 10-25mg / mL.
[0089] Through the above implementation, the drug loading effect of the developable embolic microspheres in the present invention is good, the drug loading rate can reach more than 99.3%, and the drug loading speed is fast, and the drug loading rate can reach more than 98.6% within 10 minutes.
[0090] In some embodiments of the present invention, in step S1, a polyhydroxy polymer, a developable molecule, an anionic modifier, a cross-linking agent, an active ingredient and water are mixed to obtain an aqueous phase material.
[0091] The second aspect of the present invention provides a developable embolic microsphere, which is prepared by the above-mentioned preparation method.
[0092] In some embodiments of the present invention, the particle size of the developable embolic microspheres is comprised between 50 and 1000 μm.
[0093] In some embodiments of the present invention, the particle size of the developable embolic microspheres includes 100-300 μm, 301-500 μm, 501-800 μm, etc., such as further optionally 100-150 μm, 151-300 μm, 301-500 μm, 501-800 μm, etc.
[0094] In some embodiments of the present invention, the developable embolic microspheres are loaded with active ingredients.
[0095] In some embodiments of the present invention, the developable embolic microspheres include polyvinyl alcohol chains and R connected to the polyvinyl alcohol chains via acetal structures. 3 or R 4 At least one of. Optionally, R 3 and R 4 The group is independently selected from any one of the above-mentioned developable molecules, anionic modifiers or cross-linking agents, and is formed by directly or indirectly modifying the polyvinyl alcohol chain.
[0096] In some embodiments of the present invention, the groups R on the same polyvinyl alcohol chain 3 and R 4 Several C atoms may be spaced apart, for example, more than 2 C atoms may be spaced apart.
[0097] In some embodiments of the present invention, the developable embolic microspheres may include the following structure:
[0098]
[0099] The wavy line represents the polyvinyl alcohol chain structure (the number of C is 1 or more)
[0100] In some embodiments of the present invention, R 3 , R 4 Can be independently selected from the following structures:
[0101]
[0102] a' is an integer, and 5≥1a'≥1;
[0103] W 1 ~W 2 Independently selected from C 2-5 The alkyl group may be of the chemical formula C n’ H 2n’ An alkylene group, wherein n' is an integer, and n' is 2-5;
[0104] W 3 ~W 4 Independently selected from H or an anion-containing group chain; wherein the anion-containing group chain may include: -CH 2 -CH 2 -COO - Or a group formed by polymerization of an organic acid containing an acryloyl group and / or a salt of the organic acid;
[0105] W 5 ~W 8 Independently selected from polyvinyl alcohol chains containing a plurality of Cs, wherein the number of Cs in the polyvinyl alcohol chain is 2 or more.
[0106] The third aspect of the present invention provides a chemoembolization material, comprising the above-mentioned developable embolization microspheres.
[0107] In some embodiments of the present invention, the chemoembolic material comprises an embolic agent for treating liver cancer.
[0108] The fourth aspect of the present invention provides a medical product comprising the above-mentioned chemoembolization material.
[0109] The fifth aspect of the present invention proposes the use of the above-mentioned developable embolic microspheres in the preparation of tumor diagnosis products or tumor treatment products. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:
[0111] Figure 1 is the infrared chromatogram of the developable embolic microspheres in Example 4 of the present invention;
[0112] Figure 2 The microscopic test results of the developable embolic microspheres in Example 4 of the present invention are shown in FIG. Figure 1 ;
[0113] Figure 3 The microscopic test results of the developable embolic microspheres in Example 4 of the present invention are shown in FIG. Figure 2 ;
[0114] Figure 4 This is a microscopic test result diagram of the developable embolic microspheres in Example 7 of the present invention;
[0115] Figure 5 The pictures are the development effects of the embolic microspheres and the barium sulfate powder in Examples 2 and 4 of the present invention and Comparative Example 1;
[0116] Figure 6 This is a graph showing the compression performance test results of the developable embolic microspheres in Example 4 of the present invention. DETAILED DESCRIPTION
[0117] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0118] The experimental methods in the following examples without specifying specific conditions are generally carried out according to conventional conditions in the art or conditions recommended by the manufacturers; the raw materials and reagents used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets.
[0119] The structural formulas of compounds 1-3 are:
[0120]
[0121] Example 1
[0122] This embodiment discloses a developable embolic microsphere, the preparation process of which includes the following steps:
[0123] (I) Weigh 50 g of polyvinyl alcohol 1999 and put it into 350 g of distilled water, raise the temperature to 95°C until the solution is completely clear and transparent, and then cool it to room temperature to prepare a polyvinyl alcohol solution. Take 15 g of the polyvinyl alcohol solution and add 0.455 g of compound 1, stir evenly, then add 0.826 g of glyoxylic acid and 0.18 mL of glutaraldehyde, and stir evenly at room temperature to obtain an aqueous phase.
[0124] Add 100 mL of butyl acetate and 2 g of cellulose acetate butyrate into a three-necked bottle, and stir and disperse at room temperature to obtain an oil phase.
[0125] (II) Add the aqueous phase to the oil phase, stir for 25 minutes, raise the temperature to 60°C, and react for 4 hours. After the reaction is completed, wash with butyl acetate, ethanol, PBS buffer solution, and water for 3 times each, and then sieve through a sieve to obtain microspheres in the range of 100-300μm (including particle size range: 100-150μm, 151-300μm), 301-500μm, and 501-800μm. Use a vacuum drying oven to dry the microspheres into powder to obtain the developable embolic microspheres, which are stored at room temperature in the dark for later use.
[0126] This embodiment also discloses a chemoembolization material, including the developable embolization microspheres prepared in this embodiment.
[0127] This embodiment also discloses a medical product, including the chemoembolization material in this embodiment.
[0128] In some other embodiments of the present invention, the polyvinyl alcohol may be polyvinyl alcohol 67000 or the like.
[0129] Example 2
[0130] This embodiment discloses a developable embolic microsphere, the preparation process of which includes the following steps:
[0131] (I) Weigh 80g of polyvinyl alcohol 1799 and put it into 320g of distilled water, raise the temperature to 95°C until the solution is completely clear and transparent, and then cool it to room temperature to prepare a polyvinyl alcohol solution. Take 8g of polyvinyl alcohol solution and add 0.762g of triiodobenzaldehyde. After uniform dispersion, add 0.12g of N-(2,2-dimethoxyethyl)-2-acrylamide, 1.08g of 2-acrylamide-2-methylpropanesulfonic acid and sodium 2-acrylamide-2-methylpropanesulfonate (mass ratio of 4:1), and stir at 40°C for 4 hours. Add 0.045g of potassium persulfate to the reaction system, stir evenly and obtain an aqueous phase.
[0132] 1.8 g of cellulose acetate butyrate and 100 mL of butyl acetate were added to a three-necked bottle and dissolved at 50° C. to obtain an oil phase.
[0133] (II) Add the aqueous phase to the oil phase, stir and disperse evenly for 20 minutes, then heat to 80°C and react for 6 hours. Wash the microspheres obtained after the reaction three times with butyl acetate, acetone, sodium bicarbonate solution, and purified water, and then sieve with a sieve to obtain microspheres in the range of 100-300 μm (including particle size range: 100-150 μm, 151-300 μm), 301-500 μm, and 501-800 μm. Use a vacuum drying oven to dry the microspheres into powder to obtain the developable embolic microspheres, which are stored at room temperature away from light for later use.
[0134] This embodiment also discloses a chemoembolization material, including the developable embolization microspheres prepared in this embodiment.
[0135] This embodiment also discloses a medical product, including the chemoembolization material in this embodiment.
[0136] Example 3
[0137] This embodiment discloses a developable embolic microsphere, the preparation process of which includes the following steps:
[0138] (I) Weigh 20g of pig skin gelatin and put it into 100g of distilled water, raise the temperature to 50°C until the solution is completely clear and transparent, and then cool it to room temperature to obtain a gelatin solution. Take 12g of the gelatin solution and add 1.22g of acrylic acid-sodium acrylate (mass ratio is 1:1), 0.89g of 2,3,5-triiodobenzaldehyde, 0.18g of N-(2,2-dimethoxyethyl)-2-acrylamide, and 0.03g of potassium persulfate, and stir at room temperature for 30 minutes to obtain an aqueous phase.
[0139] Add 2.2 g of cellulose acetate butyrate and 100 mL of butyl acetate into a three-necked bottle and stir evenly at 30° C. to obtain an oil phase.
[0140] (II) Add the aqueous phase to the oil phase, stir and disperse for 25 minutes, then heat to 75°C and react for 4 hours. Wash the microspheres obtained after the reaction three times with butyl acetate, ethanol, sodium bicarbonate solution, and purified water, and then sieve with a sieve to obtain microspheres in the range of 100-300 μm (including particle size range: 100-150 μm, 151-300 μm), 301-500 μm, and 501-800 μm. Use a vacuum drying oven to dry the microspheres into powder to obtain the developable embolic microspheres, which are stored at room temperature away from light for later use.
[0141] This embodiment also discloses a chemoembolization material, including the developable embolization microspheres prepared in this embodiment.
[0142] This embodiment also discloses a medical product, including the chemoembolization material in this embodiment.
[0143] Example 4
[0144] This embodiment discloses a developable embolic microsphere, the preparation process of which includes the following steps:
[0145] (Ⅰ) Weigh 50g of polyvinyl alcohol 1999 and put it into 350g of distilled water, raise the temperature to 95℃ until the solution is completely clear and transparent, then cool to room temperature to prepare a polyvinyl alcohol solution. Take 15g of polyvinyl alcohol solution and add 0.455g of compound 1, stir evenly and heat to 80℃, react for 10 hours and then cool to room temperature. Then add 0.18mL of N-(2,2-dimethoxyethyl)-2-acrylamide, 1.26g of 2-acrylamide-2-methylpropanesulfonic acid: 2-acrylamide-2-methylpropanesulfonic acid sodium (mass ratio is 4:1), and continue stirring at 50℃ for 4 hours. After cooling to room temperature, add 0.038g of sodium persulfate and stir evenly to obtain an aqueous phase.
[0146] Add 100 mL of butyl acetate and 2 g of cellulose acetate butyrate into a three-necked bottle, and stir and disperse at 60° C. to obtain an oil phase.
[0147] (II) Add the aqueous phase to the oil phase, stir for 25 minutes, add 0.5 mL of tetramethylethylenediamine and raise the temperature to 80°C for 4 hours. After the reaction is completed, wash with acetone, ethanol and water three times each, and then sieve through a sieve to obtain microspheres in the range of 100-300 μm (including particle size range: 100-150 μm, 151-300 μm), 301-500 μm, and 501-800 μm, see Figure 2-3 The microspheres were dried into powder using a vacuum drying oven to obtain the developable embolic microspheres, which were then stored at room temperature away from light for later use.
[0148] This embodiment also discloses a chemoembolization material, including the developable embolization microspheres prepared in this embodiment.
[0149] This embodiment also discloses a medical product, including the chemoembolization material in this embodiment.
[0150] In some other embodiments of the present invention, the polyvinyl alcohol may be polyvinyl alcohol 67000, polyvinyl alcohol 1788, etc.
[0151] Example 5
[0152] This embodiment discloses a developable embolic microsphere, which is different from the embodiment 4 only in that the sodium 2-acrylamide-2-methylpropane sulfonate in the embodiment 4 is replaced by 2-acrylamide-2-methylpropane sulfonic acid of equal mass.
[0153] Example 6
[0154] This embodiment discloses a developable embolic microsphere, which is different from the embodiment 4 only in that an equal mass of sodium 2-acrylamide-2-methylpropane sulfonate is used to replace the 2-acrylamide-2-methylpropane sulfonic acid in the embodiment 4.
[0155] This embodiment also discloses a chemoembolization material, including the developable embolization microspheres prepared in this embodiment.
[0156] This embodiment also discloses a medical product, including the chemoembolization material in this embodiment.
[0157] Example 7
[0158] This embodiment discloses a developable embolic microsphere, which differs from the embodiment 4 only in that 0.405 g of compound 2 is used to replace 0.455 g of compound 1 in the embodiment 4. Finally, the developable embolic microsphere is obtained, see Figure 4 .
[0159] This embodiment also discloses a chemoembolization material, including the developable embolization microspheres prepared in this embodiment.
[0160] This embodiment also discloses a medical product, including the chemoembolization material in this embodiment.
[0161] Example 8
[0162] This example discloses a developable embolic microsphere, which is different from Example 4 only in that 0.455 g of Compound 1 in Example 4 is replaced by 0.365 g of Compound 3.
[0163] This embodiment also discloses a chemoembolization material, including the developable embolization microspheres prepared in this embodiment.
[0164] This embodiment also discloses a medical product, including the chemoembolization material in this embodiment.
[0165] Comparative Example 1
[0166] This comparative example discloses an embolic microsphere, the preparation process of which comprises the following steps:
[0167] (I) Weigh 50g of polyvinyl alcohol 1788 (polyvinyl alcohol 1999 can also be used) and put it into 350g of distilled water, raise the temperature to 95°C until the solution is completely clear and transparent, and then cool it to room temperature to prepare a polyvinyl alcohol solution. Take 15g of the polyvinyl alcohol solution and add 0.18mL of N-(2,2-dimethoxyethyl)-2-acrylamide, 1.26g of 2-acrylamide-2-methylpropanesulfonic acid: 2-acrylamide-2-methylpropanesulfonic acid sodium (mass ratio is 4:1), and continue stirring at 50°C for 4 hours. After cooling to room temperature, add 0.038g of sodium persulfate and stir evenly to obtain an aqueous phase.
[0168] Add 100mL of butyl acetate and 2g of cellulose acetate butyrate to a three-necked flask, and stir and disperse at 60°C to obtain an oil phase. (II) Add the aqueous phase to the oil phase, stir for 25 minutes, then add 0.5mL of tetramethylethylenediamine and raise the temperature to 80°C for 4 hours. After the reaction is completed, wash with acetone, ethanol, and water three times each, and then sieve through a sieve to obtain microspheres in the range of 100-300μm (including particle size range: 100-150μm, 151-300μm), 301-500μm, and 501-800μm. Use a vacuum drying oven to dry the microspheres into powder and store them at room temperature away from light for later use.
[0169] The compounds 1-3 used in the above examples can be prepared by the following method:
[0170] (1) The preparation process of compound 1 (N-(dimethoxyethyl)-5-amino-2,4,6-triiodoisophthalic acid) is as follows:
[0171]
[0172] Specifically, 10 g of 5-amino-2,4,6-triiodoisophthalic acid and 20 mL of 20% sodium hydroxide solution were added to a three-necked flask, and 4 g of chloroacetaldehyde dimethyl acetal was added after dissolution, and the reaction was carried out at 70° C., nitrogen protection, and condensation reflux for 6 hours. After the reaction was completed, the obtained product was repeatedly extracted with saturated sodium bicarbonate aqueous solution / ethyl acetate (V:V=1:1), and the aqueous phase was concentrated and recrystallized in methanol to prepare the target product-Compound 1.
[0173] (2) The preparation process of compound 2 (N-(dimethoxyethyl)-5-amino-4,6-diiodo-1,3-phthalic acid) is as follows:
[0174]
[0175] Specifically, 10 g of 5-amino-4,6-diiodo-1,3-benzenedicarboxylic acid and 20 mL of 20% sodium hydroxide solution were added to a three-necked flask, and 5 g of chloroacetaldehyde dimethyl acetal was added after dissolution, and the reaction was carried out at 70° C., nitrogen protection, and condensation reflux for 6 hours. After the reaction was completed, the obtained product was repeatedly extracted with saturated sodium bicarbonate aqueous solution / ethyl acetate (V:V=1:1), and the aqueous phase was concentrated and recrystallized in methanol to prepare the target product-compound 2.
[0176] (3) The preparation process of compound 3 (N-(dimethoxyethyl)-3-amino-2,4,6-triiodobenzoic acid) is as follows:
[0177]
[0178] Specifically, 10 g of 3-amino-2,4,6-triiodobenzoic acid and 20 mL of 20% sodium hydroxide solution were added to a three-necked flask, and 5.5 g of chloroacetaldehyde dimethyl acetal was added after dissolution, and the reaction was carried out at 70° C., nitrogen protection, and condensation reflux for 6 hours. After the reaction was completed, the obtained product was repeatedly extracted with saturated sodium bicarbonate aqueous solution / ethyl acetate (V:V=1:1), and the aqueous phase was concentrated and recrystallized in methanol to prepare the target product-compound 3.
[0179] Test example
[0180] This test example tests the performance of the developable emboli obtained in the example, the embolic microspheres obtained in the comparative example, and the commercially available product 1-Embosphere embolic microspheres and the commercially available product 2-HepaSphere embolic microspheres, including:
[0181] (1) The infrared spectrum test of the developable embolic microspheres prepared in Example 4 was performed. The test results are as follows: Figure 1 As shown, it can be seen that a strong 511cm -1 The CI stretching vibration of was observed, indicating that the developable molecules were successfully modified on the polyvinyl alcohol.
[0182] (2) Microsphere development performance test
[0183] The test method includes: taking the prepared developable embolic and embolic microspheres with a particle size of 100-300 μm, swelling them with physiological saline, and then mixing them evenly with agar at a volume fraction of 50%. Similarly, single agar and 50% barium sulfate / agar samples are used as controls. All samples are placed in Micro CT (vivaCT80, Switzerland) for development scanning, and the development degree is calculated based on the HU of pure water being 0 and the HU of air being -1000. The test results are shown in Table 1 below, and the development photos are shown in Figure 5 As shown: Figure 5 (a) is a picture of the embolic microsphere development effect of comparative example 1; Figure 5 (b) is a picture of the developing effect of the developable embolic microspheres in Example 2; Figure 5 (c) is a picture of the developing effect of the developable embolic microspheres in Example 4; Figure 5 (d) is a picture of the development effect of barium sulfate powder;
[0184] The modification rate of the developable molecules on the polyvinyl alcohol is determined by measuring the developer concentration in the reaction solution at the start and end of the reaction with an ultraviolet spectrophotometer at 254 nm, thereby calculating the reaction modification rate.
[0185] Table 1 Embolization microsphere imaging performance test results
[0186]
[0187] As shown in Table 1 above, the developable microspheres synthesized using acrylamide-based acidic monomers have a smooth surface, while the developable microspheres obtained using aldehyde-containing monomers have a relatively rough surface. It is speculated that the possible reason is that both aldehyde-containing acid (such as glyoxylic acid in Example 1) and acetal-containing developers (such as compound 1 in Example 1) need to react with the hydroxyl group of polyvinyl alcohol, which easily leads to a decrease in the uniformity of the reaction between aldehyde-containing acid and acetal-containing developers and polyvinyl alcohol, resulting in a rough surface of the final microspheres. At the same time, it can also be seen that the development effect of the microspheres is related to the iodine content per unit volume, which is consistent with the actual theory.
[0188] (3) Microsphere compression performance test
[0189] The test method includes: taking the prepared developable embolic microspheres with a particle size of 301-800μm (including 301-500μm, 501-800μm), embolic microspheres and commercially available products 1-2 and re-swelling them with physiological saline, placing the completely swollen microspheres on the test bench, and pressing the test probe at a speed of 0.2mm / s until the compression distance reaches 20%, 50% and 80% of the microsphere diameter. If the microspheres are not broken and can be restored after being pressed to the specified degree, it is recorded as passed, otherwise it is recorded as failed if they are damaged or fail to rebound. The test results are shown in Table 2 below, where the test results of the microsphere compression performance in Example 4 are shown in Table 2. Figure 6 Shown: The left picture is before compression, the middle picture is the compressed state, and the right picture is after compression.
[0190] Table 2. Compression performance test results of embolic microspheres
[0191] Test samples Compression ratio 20% Compression ratio 50% Compression ratio 80% Example 1 pass pass Not passed Example 2 pass pass pass Example 3 pass pass pass Example 4 pass pass pass Example 7 pass pass pass Example 8 pass pass pass Comparative Example 1 pass pass pass Commercially available products 1 pass pass Not passed Commercially available product 2 pass Not passed Not passed
[0192] As can be seen from the above table, the developable embolic microspheres prepared by the present invention have excellent compression performance, which is beneficial to the occlusion effect on the target blood vessels. Compared with the use of glyoxylic acid as an anion modifier in Example 1, the use of organic acids and their corresponding salts as anion modifiers in Examples 2-4, 7-8, and the obtained developable embolic microspheres have better compression performance.
[0193] (4) Microsphere drug loading test
[0194] The test method includes: taking the above-mentioned embodiments and comparative examples to prepare developable embolic microspheres with a particle size of 150-300 μm, embolic microspheres and commercially available products 1-2, re-swelling them with physiological saline, and then taking 1 mL of microspheres into a vial using a measuring cylinder. Add 2 mL of a 20 mg / mL doxorubicin hydrochloride aqueous solution thereto, and use an ultraviolet spectrophotometer to detect the drug concentration at a wavelength of 483 nm. The test results are shown in Table 3 below:
[0195] Table 3 Table of drug adsorption rate of embolic microspheres
[0196]
[0197] From the drug adsorption rate table, it can be seen that compared with the commercially available drug-loaded microspheres, the drug loading rate of the developable embolic microspheres of the present invention is significantly improved, and the drug loading rate of the microspheres can reach more than 85% within 10 minutes. And by comparing with Comparative Example 1, it can be seen that the drug loading performance of the developable embolic microspheres of the present invention is excellent, and after the developable molecules are modified by polyhydroxy polymers, the drug loading rate of the microspheres is improved. It is speculated that the reason may be that the modified part of the developable molecules on the polyhydroxy polymer plays a supporting role in the internal structure of the microspheres, thereby forming a more unobstructed gap inside the microspheres, which is conducive to the adsorption and penetration of drugs.
[0198] (5) Microsphere stability test
[0199] The test method includes: the developable embolic microspheres with a particle size of 100-300 μm prepared in Example 4 are swollen with physiological saline, sterilized with wet heat (121°C, 30 min), and then placed at 37°C and protected from light. Part of the microspheres are taken out every 10 days and their various properties are tested. The test results are shown in Table 4 below:
[0200] Table 4 Microsphere stability test results
[0201]
[0202]
[0203] As can be seen from the above, the developable embolic microspheres in the present invention have excellent development stability, and the HU value has not been significantly weakened after being placed for 30 days, and the 30-minute drug loading rate is as high as 99.1% or more. When the developable embolic microspheres of the present invention are used for TACE surgery, it is beneficial to visualize monitoring and operation during and after the operation, allowing doctors to better judge the distribution of microsphere embolism, which is beneficial for subsequent diagnosis and treatment arrangements, and patients can also understand the treatment status more clearly, reducing patient concerns.
[0204] (6) Microsphere cytotoxicity test
[0205] The test method includes: the developable embolic microspheres with a particle size of 100-300 μm prepared in Example 4 are swollen with PBS buffer, and after wet heat sterilization (121°C, 30 min), the microspheres, storage solution (i.e., physiological saline during immersion) and culture medium are mixed respectively to obtain culture medium + microspheres and culture medium + storage solution groups, and then the above two groups are used to culture cells (mouse embryonic fibroblasts). The pure culture medium group was used as a control, and the CCK-8 method was used to detect cytotoxicity. The test showed that the microspheres prepared by the present invention have low cytotoxicity and good biocompatibility. The specific results are shown in Table 5 below:
[0206] Table 5 Microsphere cytotoxicity test results
[0207]
[0208] In summary, the present invention discloses a drug-loaded embolic microsphere for X-ray development, wherein a developable molecule is modified on a polyhydroxy polymer, an anionic modifier is modified on a polyhydroxy polymer or a polyhydroxy polymer modified with a developable molecule, and then a polymerization reaction is performed to obtain a developable embolic microsphere. The developable embolic microsphere prepared by the present invention has excellent X-ray development effect, drug loading performance, etc., and can be used for embolic therapy of tumor sites. Optionally, an acid-containing monomer compound (such as an anionic modifier) can be used as a catalyst to promote the reaction of an aldehyde / acetal-containing polyiodobenzene compound and an aldehyde / acetal-containing cross-linking agent (such as a bifunctional small molecule cross-linking agent) with a polyhydroxy high molecular polymer to synthesize an X-ray developable polymer intermediate, and then the acid-containing monomer compound continues to promote the cross-linking of the polymer intermediate in an oil-in-water suspension polymerization system, and participates in a polymerization reaction with salts (such as salts corresponding to the acid-containing monomer compound, persulfate) to form microspheres. Alternatively, the polymer is mixed with a developable molecule and a crosslinking agent, and reacted under the catalysis of an organic acid containing an unsaturated functional group (such as 2-acrylamido-2-methylpropanesulfonic acid); and the organic acid can also be added to the reaction system to promote the modification of anions on the polymer, and finally prepare drug-loaded embolic microspheres that can be developed by X-rays. The entire preparation process is simple and easy to operate, and no other acid is required as a catalyst, and the process of neutralization with alkali is also reduced.
[0209] The present invention uses monomers with acid catalysis to catalyze the reaction (developable molecule modification, anion modifier modification), reducing the use of other catalysts or auxiliary reagents, making the synthesis process simpler and the operation more convenient, thereby reducing cost loss and the time required for preparation and post-processing. More importantly, the microspheres synthesized using this method have better uniformity and a high degree of reaction. The finally obtained developable embolic microspheres have good X-ray development effect, drug loading performance, etc., and have good application prospects.
[0210] It should be noted that the "room temperature" in this article, unless otherwise specified, is about 20-27°C; the meaning of "about" in numerical values in this article is an error of ±2%. Unless otherwise specified, the "molecular weight" in this article refers to the "weight average molecular weight".
[0211] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing developable embolic microspheres, characterized in that: The steps include: S1, mixing a polyhydroxy polymer, a developable molecule, an anionic modifier, a crosslinking agent and water to obtain an aqueous phase material; S2, mixing the aqueous phase material with the oil phase material, polymerizing, and obtaining the developable embolic microspheres; The embolic microspheres are obtained by covalently modifying the developable molecules on the polyhydroxy polymer and reacting with raw materials including a crosslinking agent through polymerization reaction; the reaction of modifying the developable molecules on the polyhydroxy polymer includes at least one of an acetal reaction or an acetal exchange reaction; the developable molecules include at least one of N-(dimethoxyethyl)-5-amino-2,4,6-triiodoisophthalic acid, N-(dimethoxyethyl)-3-amino-2,4,6-triiodobenzoic acid or N-(dimethoxyethyl)-5-amino-4,6-diiodo-1,3-phthalic acid; In the preparation method, after both the developable molecule and the anion modifier are modified on the polyhydroxy polymer, a polymerization reaction is carried out; the anion modifier is 2-acrylamide-2-methylpropane sulfonic acid and sodium 2-acrylamide-2-methylpropane sulfonate; the mass ratio of the 2-acrylamide-2-methylpropane sulfonic acid to the sodium 2-acrylamide-2-methylpropane sulfonate is (0.5-10):1; The mass ratio of the polyhydroxy polymer to the anionic modifier includes 1:(0.05-8); the mass ratio of the polyhydroxy polymer to the developable molecule includes 1:(0.01-1.5).
2. The method for preparing developable embolic microspheres according to claim 1, characterized in that: The polyhydroxy polymer includes at least one of polyvinyl alcohol, gelatin, polysaccharide, polyvinyl alcohol derivative, gelatin derivative or polysaccharide derivative.
3. The method for preparing developable embolic microspheres according to claim 1, characterized in that: The polyhydroxy polymer includes at least one of a 1,2-diol structure and a 1,3-diol structure.
4. The method for preparing developable embolic microspheres according to claim 1, characterized in that: The molecular weight of the polyhydroxy polymer is comprised between 10,000 and 300,000.
5. The method for preparing developable embolic microspheres according to claim 1, characterized in that: The modification rate of the developable molecules on the polyhydroxy polymer is 60-85%.
6. The method for preparing developable embolic microspheres according to claim 1, characterized in that: The reaction of modifying the polyhydroxy polymer or / and the polyhydroxy polymer modified with the developable molecule with the anion modifier comprises at least one of acetalization reaction, acetal exchange reaction or cross-linking reaction.
7. The method for preparing developable embolic microspheres according to claim 1, characterized in that: The functional group in the cross-linking agent is selected from at least one of an aldehyde group, an acetal group or an acryloyl group.
8. The method for preparing developable embolic microspheres according to claim 7, characterized in that: The cross-linking agent includes at least one of glutaraldehyde, formaldehyde, N-(2,2-dimethoxyethyl)-2-acrylamide or N-(2,2-diethoxyethyl)-2-acrylamide.
9. The method for preparing developable embolic microspheres according to claim 1, characterized in that: In step S1 : a polyhydroxy polymer is mixed with water to obtain a polyhydroxy polymer solution, which is then mixed with a developable molecule, an anionic modifier and a cross-linking agent.
10. The method for preparing developable embolic microspheres according to claim 1, characterized in that: Step S1 comprises the following steps: mixing the polyhydroxy polymer solution with developable molecules, anionic modifiers and cross-linking agents, and then adding persulfate to obtain the aqueous phase material.
11. The method for preparing developable embolic microspheres according to claim 1, characterized in that: The preparation method further comprises step S3: mixing the developable embolic microspheres obtained in step S2 with active ingredients to obtain developable embolic microspheres loaded with the active ingredients.
12. A developable embolic microsphere, characterized in that: The method is prepared by any one of claims 1 to 11.
13. The developable embolic microspheres according to claim 12, characterized in that: The particle size of the developable embolic microspheres is 50-1000 μm.
14. A chemoembolization material, characterized in that: The method comprises the developable embolic microspheres as described in any one of claims 12 to 13.
15. A medical product, characterized in that: Comprising the chemoembolization material according to claim 14.
16. Use of the developable embolic microspheres according to any one of claims 12 to 13 in the preparation of tumor diagnosis products or tumor treatment products.
Citation Information
Patent Citations
Developing embolism microsphere for treating tumor diseases through minimally invasive interventional therapy and preparation method thereof
CN106822983A